Specific Process Knowledge/Etch/DRIE/Pegasus-3/DREM/DREM 0.5kW v2.3: Difference between revisions

From LabAdviser
Jmli (talk | contribs)
Created page with "{| border="2" cellpadding="0" cellspacing="0" style="text-align:center;" |- ! rowspan="2" width="40"| Date ! colspan="2" width="120"| Substrate Information ! colspan="4" | Pro..."
 
Jmli (talk | contribs)
No edit summary
Line 17: Line 17:
|-
|-
|16/6-2021
|16/6-2021
|PegReticle wafer
|150 mm wafer with standard DUV resist and PegReticle pattern
|Si /  25-50%
|Si /  25-50%
|C06692.03 pegreticle wafer
|C06692.03 pegreticle wafer

Revision as of 15:23, 2 December 2021

Date Substrate Information Process Information Results
Wafer info Material/ Exposed area Condi- tioning Recipe Wafer ID Comments SEM images Picoscope Numbers
16/6-2021 150 mm wafer with standard DUV resist and PegReticle pattern Si / 25-50% C06692.03 pegreticle wafer nanolab/ jmli / DREM / DREM 0.5kW v2.3, 50 cycles or 4:35 minutes C06694.01 Process log entry

SEM image: c155 c157 c153
Trench width (um) 0.21 0.79 0.84
Etched depth (um) 1.08 1.27 1.41
Etch rate (um/min) 0.24 0.28 0.31
Etch rate (nm/cyc) 21.61 25.46 28.14
Sidewall bowing (%) 0 1 0
Sidewall angle (degs) 90.31 90.19 90.3
Bottom bowing (%) 40.66 22.98 21.46
Aspect ratio 5.04 1.6 1.67
16/6-2021 Morten Foss wafer Si / 10% C06695.14 nanolab/ vy / DREM / DREM 0.5 kW v2.3 75 cyc or 6:52.5 mins C06694.01 Process log entry

SEM image:
Trench width (um)
Etched depth (um)
Etch rate (um/min)
Etch rate (nm/cyc)
Sidewall bowing (%)
Sidewall angle (degs)
Bottom bowing (%)
Aspect ratio
27/9-2021 DUV litho wafer, Si / 25-50% C06873.01 nanolab/ jmli / DREM / DREM 0.5kW peg3, 100 cycles or 9:10 minutes C06873.02 30 sec O2 0.2kW barcProcess log entry

SEM image: c157 c158 c159 c161 c162 c160 c156 c163
Trench width (um) 0.17 0.22 0.25 0.42 0.43 0.52 0.55 2.03
Etched depth (um) 1.3 1.36 1.4 1.56 1.57 1.62 1.64 1.87
Etch rate (um/min) 0.14 0.15 0.15 0.17 0.17 0.18 0.18 0.2
Etch rate (nm/cyc) 13 14 14 16 16 16 16 19
Sidewall bowing (%) 0 0.2 0.2 0.3 0.4 0.1 -0.1 0.1
Sidewall angle (degs) 89.38 89.33 89.41 89.29 89.43 89.44 89.4 89.21
Bottom bowing (%) 34.34 24.69 27.76 23.55 22.1 20.81 23.56 11.77