Jump to content

Specific Process Knowledge/Wafer and sample drying/Critical Point Dryer: Difference between revisions

From LabAdviser
Kn (talk | contribs)
New page: '''Critical Point Dryer''' The critical point dryer is used to dry fragile structures that may be damaged in a normal drying procedure. Fragile structures may be thin membranes, or free h...
 
Kn (talk | contribs)
No edit summary
Line 1: Line 1:
'''This page is under construction and the values and data below are not all correct right now./ KN'''
'''Critical Point Dryer'''
'''Critical Point Dryer'''


Line 6: Line 8:




Purpose Drying of wafers or chips To dry fragile structures (example membranes, grippers, cantilevers).
{| border="2" cellspacing="0" cellpadding="10"
|-
!style="background:silver; color:black;" align="left"|Purpose  
|style="background:LightGrey; color:black"|Drying of wafers or chips
|style="background:WhiteSmoke; color:black"|
To dry fragile structures (example membranes, grippers, cantilevers).
|-
|-
!style="background:silver; color:black" align="left" valign="top" rowspan="3"|Process parameter range
|style="background:LightGrey; color:black"|Process Temperature
|style="background:WhiteSmoke; color:black"|
*Room temperature to 500<math>\rm{^o}</math>C
|-
|style="background:LightGrey; color:black"|Process pressure
|style="background:WhiteSmoke; color:black"|
*~5<math>\cdot</math>10<sup>-4</sup>mbar - 2000mbar
|-
|style="background:LightGrey; color:black"|Piston Force
|style="background:WhiteSmoke; color:black"|
*Depending on the area, for 4" wafers 200-20000N.
|-
!style="background:silver; color:black" align="left" valign="top" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Batch size
|style="background:WhiteSmoke; color:black"|
*One 4" or 6" wafer per run
*Pieces are only allowed with speciel permission 
|-
| style="background:LightGrey; color:black"|Substrate material allowed
|style="background:WhiteSmoke; color:black"|
*Silicon wafers
*Quartz wafers
*Pyrex wafers
|-
| style="background:LightGrey; color:black"|Material allowed on the substrate
|style="background:WhiteSmoke; color:black"|
*Silicon oxide
*Silicon (oxy)nitride
*Poly Silicon
*Photoresist
*PMMA
*TOPAS
*SU-8
*Metals: Au, Sn, Ag, Al, Ti.
|-
|}
 
 
Process parameter range Process Temperature 0 oC temperature to 45oC  
Process parameter range Process Temperature 0 oC temperature to 45oC  
Process pressure 1 atm to (maximum) 95 atm (1400 PSI)
Process pressure 1 atm to (maximum) 95 atm (1400 PSI)

Revision as of 11:55, 17 February 2010

This page is under construction and the values and data below are not all correct right now./ KN

Critical Point Dryer

The critical point dryer is used to dry fragile structures that may be damaged in a normal drying procedure. Fragile structures may be thin membranes, or free hanging structures like cantilevers and grippers.

In the critical point dryer, these structures are dried in CO2. In the drying process, the sample is first put into Isopropanol, and loaded into the machine. In the process itself, the isopropanol is exchanged for liquid CO2. When there is only CO2 in the machine, the pressure and temperature in the chamber is raised, above the so called “critical point”. In this way, there is never a liquid/gas interface, but instead the liquid is turned into a mixture of equal parts of gas and liquid. Because of this, the problem with surface tension, which destroys the fragile structures through capillary forces, is avoided.


Purpose Drying of wafers or chips

To dry fragile structures (example membranes, grippers, cantilevers).

Process parameter range Process Temperature
  • Room temperature to 500oC
Process pressure
  • ~5⋅10-4mbar - 2000mbar
Piston Force
  • Depending on the area, for 4" wafers 200-20000N.
Substrates Batch size
  • One 4" or 6" wafer per run
  • Pieces are only allowed with speciel permission
Substrate material allowed
  • Silicon wafers
  • Quartz wafers
  • Pyrex wafers
Material allowed on the substrate
  • Silicon oxide
  • Silicon (oxy)nitride
  • Poly Silicon
  • Photoresist
  • PMMA
  • TOPAS
  • SU-8
  • Metals: Au, Sn, Ag, Al, Ti.


Process parameter range Process Temperature 0 oC temperature to 45oC Process pressure 1 atm to (maximum) 95 atm (1400 PSI) Substrates Batch size 1 to 5 wafers per run. Sizes: 2”, 4" or 6"

	or
	Pieces (up to 10x10mm) 

Substrate material allowed Silicon wafers

	Quartz wafers 
	Pyrex wafers 
	InAlP
	GaAs

Material allowed on the substrate Silicon oxide

	Silicon nitride 
	Poly Silicon 
	SU-8 


Comparison of samples dried in air and with Critical Point Dryer

This shows a comparison of samples that have been dried in the critical point dryer, and samples that have been dried in air. Below are pictures of two wafers that have been prepared in the same way- but dried with different methods after the final etching step. Cantilevers of SiN, up to 710 µm long and 100 µm wide, are fabricated in the etching step. The thickness of the cantilevers is about 0.5 µm


After drying wafers in air, the majority of the cantilevers are bended and sticking to the underlying surface.

Pic 1 Dried in air: most cantilevers are bended.

Pic 2 Dried with Critical Point Dryer. The cantilevers are free hanging, and have not bended. The dimensions of the cantilevers are 100 x 710 µm, and the thickness is about 0.5 µm.

Pic 3 Dried with the Critical Point Dryer. The cantilevers structures are free hanging after the drying.


An acknowledgment goes to Tom Larsen, Nanoprobes, DTU Nanotech, who provided the pictures.