Specific Process Knowledge/Thin film deposition/Deposition of Silicon Oxide: Difference between revisions
Line 34: | Line 34: | ||
![[Specific Process Knowledge/Thin film deposition/Furnace LPCVD TEOS|LPCVD(TEOS)]] | ![[Specific Process Knowledge/Thin film deposition/Furnace LPCVD TEOS|LPCVD(TEOS)]] | ||
![[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] | ![[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] | ||
![[Specific Process Knowledge/Thin film deposition/Lesker|Sputter System Lesker]] | ![[Specific Process Knowledge/Thin film deposition/Lesker|Sputter System Lesker]] | ||
![[Specific Process Knowledge/Thin film deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system|Sputter-system Metal-Oxide(PC1)]] | ![[Specific Process Knowledge/Thin film deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system|Sputter-system Metal-Oxide(PC1)]] | ||
Line 44: | Line 43: | ||
!General description | !General description | ||
|Low Presure Chemical Vapor Deposition TEOS gives a good quality SiO2 and is a batch process. | |Low Presure Chemical Vapor Deposition TEOS gives a good quality SiO2 and is a batch process. | ||
|Plasma Enhanced Chemical Vapor Deposition has the advantage that a silicon oxide and be deposited with a quit high deposition rate at a rather low temperature | |Plasma Enhanced Chemical Vapor Deposition has the advantage that a silicon oxide and be deposited with a quit high deposition rate at a rather low temperature | ||
|Sputter deposition: can be done on top of a large range of materials | |Sputter deposition: can be done on top of a large range of materials | ||
|Sputter deposition: can be done on top of a large range of materials. | |Sputter deposition: can be done on top of a large range of materials. | ||
Line 59: | Line 57: | ||
*Si<sub>x</sub>O<sub>y</sub>H<sub>z</sub> | *Si<sub>x</sub>O<sub>y</sub>H<sub>z</sub> | ||
Can be doped with boron, phosphorus or germanium | Can be doped with boron, phosphorus or germanium | ||
| | | | ||
* | * | ||
Line 76: | Line 72: | ||
| | | | ||
*~40 nm - 30 µm | *~40 nm - 30 µm | ||
| | | | ||
* Thin layers (up to 200-300 nm) | * Thin layers (up to 200-300 nm) | ||
Line 92: | Line 86: | ||
| | | | ||
*300 °C | *300 °C | ||
| | | | ||
*Room temp to 400 °C | *Room temp to 400 °C | ||
Line 111: | Line 103: | ||
*Less good | *Less good | ||
*When doped with phosphorus and/or Boron the oxide can float at about 1000 °C in a wet oxidation. | *When doped with phosphorus and/or Boron the oxide can float at about 1000 °C in a wet oxidation. | ||
*Deposition on one side of the substrate | *Deposition on one side of the substrate | ||
| | | | ||
Line 133: | Line 122: | ||
*Less dense film | *Less dense film | ||
*Incorporation of hydrogen in the film | *Incorporation of hydrogen in the film | ||
| | | | ||
* | * | ||
Line 154: | Line 141: | ||
*1-3 100 mm wafers | *1-3 100 mm wafers | ||
*1 150 mm wafer | *1 150 mm wafer | ||
| | | | ||
*Pieces or | *Pieces or | ||
Line 187: | Line 168: | ||
*IIIV materials (in PECVD2) | *IIIV materials (in PECVD2) | ||
*Small amount of metal (in PECVD3) | *Small amount of metal (in PECVD3) | ||
| | | | ||
* Silicon | * Silicon |
Revision as of 10:32, 21 April 2022
Feedback to this page: click here
Deposition of Silicon Oxide can be done with either LPCVD, PECVD, by sputter technique or ALD. You can also make a silicon oxide layer by growing a thermal oxide in a hot furnace but that requires a silicon surface as a starting point.
Deposition of Silicon Oxide using LPCVD
The LPCVD oxide you can deposit at DTU Nanolab is called TEOS oxide. It can be made in the LPCVD TEOS furnace. It is a batch process meaning you can run a batch of 13 wafers at a time. The deposition takes place at temperatures of 725 degrees Celsius. The TEOS oxide has good step coverage and hole filing/covering properties and the film thickness is very uniform over the wafer. We have two standard TEOS processes: One for depositing standard layers ~(0-1.5 µm) and one for deposition thick layers ~(1.5µm-4µm). The TEOS oxide has a dielectric constant very close to the one for thermal oxide (3.65 for TEOS).
Deposition of Silicon Oxide using PECVD
PECVD oxide can be deposited in one of the PECVD systems. You can run 1-3 wafers at a time depending on which one of the PECVD's you use. The deposition takes place at 300 degrees Celcius. This can be of importance for some applications but it gives a less dense film and the oxide is expected to have some hydrogen incorporated. The step coverage and thickness uniformity of the film is not as good as for the LPCVD TEOS oxide. PECVD oxide has excellent floating properties when doped with boron and/or phosphorus. Then it can be used eg. as top cladding for waveguides or encapsulation of various structures/components. In one of our PECVD systems (PECVD3) we allow small amounts of metal on the wafers entering the system, this is not allowed in the LPCVD and in PECVD4.
Deposition of Silicon Oxide using sputter deposition technique
At DTU Nanolab you can also deposit silicon oxide using the Sputter-System (Lesker), the Sputter-System Metal Oxide(PC1) or the IBE Ionfab300 sputter system. One of the advantages here is that you can deposit on many kinds of material.
- Reactively Sputtered Silicon Oxide in Sputter-System Metal Oxide (PC1)
- Deposition of Silicon Oxide using Lesker sputter tool
- Deposition of Silicon Oxide using IBE/IBSD Ionfab300
- Deposition conditions in Sputter-System Metal Oxide(PC1)
Deposition of Silicon Oxide using ALD
Thin films of silicon oxide up to 50 nm can also be deposited in the ALD2. The ALD2 uses the plasma source and can therefore only deposit on one wafer at a time. The deposition takes place at 300 oC, where the growth rate is 0.1222nm on flat samples. It is also possible to deposit uniform layers on high aspect ratio structures with a growth rate of 0.1629 nm/cycle.
Comparison of the methods for deposition of Silicon Oxide
LPCVD(TEOS) | PECVD | Sputter System Lesker | Sputter-system Metal-Oxide(PC1) | ALD2 | |
---|---|---|---|---|---|
General description | Low Presure Chemical Vapor Deposition TEOS gives a good quality SiO2 and is a batch process. | Plasma Enhanced Chemical Vapor Deposition has the advantage that a silicon oxide and be deposited with a quit high deposition rate at a rather low temperature | Sputter deposition: can be done on top of a large range of materials | Sputter deposition: can be done on top of a large range of materials. | Atomic Layer deposition provides an uniform layer with a good covering even on high aspect ratio structures. |
Stochiometry |
|
Can be doped with boron, phosphorus or germanium |
|
|
|
Film thickness range |
|
|
|
|
|
Process Temperature |
|
|
|
|
|
Step Coverage |
|
|
|
|
|
Film Quality |
|
|
|
|
|
Substrate size / Batch size |
|
|
|
|
|
Allowed materials |
|
|
|
|
|