Line 117: Line 117:
|
|
*~75 nm/min (Thermal oxide) in BHF
*~75 nm/min (Thermal oxide) in BHF
*~90 nm/min (Thermal oxide) in SIO Etch
*~80 nm/min (Thermal oxide) in BOE 7:1 Etchant VLSI with Surfactant
*~25 nm/min (Thermal oxide) in 5%HF
*~25 nm/min (Thermal oxide) in 5%HF
*~3-4µm/min in 40%HF
*~3-4µm/min in 40%HF

Revision as of 14:38, 19 October 2021

Feedback to this page: click here

Comparing silicon oxide etch methods at DTU Nanolab

There are a broad varity of silicon oxide etch methods at DTU Nanolab. The methodes are compared here to make it easier for you to compare and choose the one that suits your needs.

Compare the methods for Silicon Oxide etching

Wet Silicon Oxide etch (BHF/HF) ASE III-V RIE AOE (Advanced Oxide Etch) DRIE Pegasus 4 ICP metal IBE/IBSD Ionfab 300 HF Vapour Phase Etch
Generel description
  • Isotropic etch
  • Anisotropic etch: vertical sidewalls
  • Anisotropic etch: vertical sidewalls
  • Premarily for III-V samples
  • Anisotropic etch: vertical sidewalls
  • Anisotropic etch: almost vertical sidewalls
  • Anisotropic etch: almost vertical sidewalls
  • We prefer that SiO2 etch on 6" wafers takes place in the Pegasus 4.
  • Primarily for pure physical etch by sputtering with Ar-ions
  • Gas phase HF etching with ethanol as carrier
Possible masking materials
  • Photoresist
  • PolySilicon
  • Silicon nitride (LPCVD)
  • Blue film
  • Cr/Au for deeper etches (plastic beaker)
  • Photoresist
  • DUV resist
  • E-beam resist
  • Silicon
  • Silicon Nitride
  • Metals if they cover less than 5% of the wafer area
  • Photoresist
  • DUV resist
  • E-beam resist
  • Aluminum
  • Silicon
  • Silicon Nitride
  • Photoresist
  • DUV resist
  • E-beam resist
  • Silicon
  • Silicon Nitride
  • Aluminium
  • Chromium (Please try to avoid this)
  • Photoresist
  • DUV resist
  • E-beam resist
  • Si
  • Silicon Nitride
  • Chromium (ask for permission)
  • Photoresist
  • DUV resist
  • E-beam resist
  • Si
  • Silicon Nitride
  • Aluminium
  • Chromium
  • Ti
  • Any material that is accepted in the machine
  • Aluminium
  • Aluminium oxide
  • Polysilicon
Etch rate range
  • ~75 nm/min (Thermal oxide) in BHF
  • ~80 nm/min (Thermal oxide) in BOE 7:1 Etchant VLSI with Surfactant
  • ~25 nm/min (Thermal oxide) in 5%HF
  • ~3-4µm/min in 40%HF
  • Process dependent
  • Tested range: ~20nm/min - ~250nm/min
  • Process dependent
  • Tested range: ~1nm/min - ~30nm/min
  • Process dependent
  • Tested range: ~60nm/min - ~550nm/min
  • Process dependent

<500nm/min

  • Process dependent
  • Tested range: ~40nm/min - ~200nm/min
  • Process dependent
  • Tested once ~22nm/min
  • Sample and load dependent
  • Expected range: 12 - 175 nm/min
Substrate size
  • #1-25 100mm wafers in our 100mm bath
  • What can be fitted in a plastic beaker
  • As many small samples as can be fitted on the 100mm carrier (bad/no cooling!).
  • #1 100mm wafer (or smaller with carrier)
  • #1 150mm wafer (only when set up for 150mm)
  • Up to 20cm in diameter
  • As many small samples as can be fitted on a 100mm wafer
  • #1 50 mm wafer fitted on a 100mm wafer
  • #1 100 mm wafer
  • #1 150 mm wafers (only when the system is set up to 150mm)
  • As many small samples as can be bonded on a 150mm wafer
  • #1 50 mm wafer bonded on a 150mm wafer
  • #1 100 mm wafer bonded on a 150nm wafer
  • #1 150 mm wafers
  • As many small samples as can be fitted on a 150mm wafer
  • #1 50 mm wafer fittesd on a 150mm wafer
  • #1 100 mm wafer fitted on a 150nm wafer
  • #1 150 mm wafers
  • As many samples as can be securely fitted on a up to 200mm wafer
  • #1 50 mm wafer with special carrier
  • #1 100 mm wafer with special carrier
  • #1 150 mm wafers with special carrier
  • #1 200 mm wafer
  • Pieces
  • #1 50 mm wafer
  • #1 100 mm wafer
  • #1 150 mm wafer
Allowed materials

In the dedicated bath:

  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • Blue film

In a plastic beaker:

  • No limits cross contamination wise