'''The plasma:'''<br>
'''The plasma:'''<br>
The plasma emits light as the gas constituents are continuously exited
Inside the process chamber, the RF field will cause electrons to get pulled off the gas atoms to form ions, radicals and free, fast moving electrons. As the electrons bounce into the gas constituents, they latter are pushed into excited states from which they may decay under emission of photons.
These photons typically have an energy in the visible range and hence the plasma emits light at certain wavelengths
 
 
The plasma in the process chamber emits light; the RF field
that depends on what molecules are in the
as the gas constituents are continuously pumped into excited rotational


=fdgsdfg=
=fdgsdfg=

Revision as of 14:50, 26 November 2020

Optical endpoint detection on the dry etch tools at DTU Nanolab

Several dry etch tools at DTU Nanolab are equipped with an endpoint detection system. Out of those systems only one is not of the type optical endpoint detection. The instruments are:

  • ICP Metal Etch
  • III-V ICP
  • Pegasus 1
  • Pegasus 4

The section below describes the principle behind the optical endpoint detection system.

Optical Emission Spectroscopy

The etch process:
As an example, let's take the etching of silicon by fluorine in one of the dry etchers. The fluorine is supplied to the system as SF6 gas that is fed to the process chamber using mass flow controllers. Driven by the RF generators (both coil and platen) the plasma will decompose the gas in a series of dissociation and ionisation reactions to form fluorine radicals F*. In the areas on the wafer that are not covered by a mask, the exposed silicon atoms will be attacked aggressively by the fluorine radical to form volatile SiF. As such, the SiF will desorp from the wafer surface and eventually get pumped away.

The plasma:
Inside the process chamber, the RF field will cause electrons to get pulled off the gas atoms to form ions, radicals and free, fast moving electrons. As the electrons bounce into the gas constituents, they latter are pushed into excited states from which they may decay under emission of photons. These photons typically have an energy in the visible range and hence the plasma emits light at certain wavelengths


The plasma in the process chamber emits light; the RF field

that depends on what molecules are in the
as the gas constituents are continuously pumped into excited rotational

fdgsdfg

Monitored species Wavelength (nm) Monitored species Wavelength (nm)
Al 308.2, 309.3, 396.1 In 325.6
AlCl 261.4 N 674.0
As 235.0 N2 315.9, 337.1
C2 516.5 NO 247.9, 288.5, 289.3, 303.5, 304.3, 319.8, 320.7, 337.7, 338.6
CF2 251.9 O 777.2, 844.7
Cl 741.4 OH 281.1, 306.4, 308.9
CN 289.8, 304.2, 387.0 S 469.5
CO 292.5, 302.8, 313.8, 325.3, 482.5, 483.5, 519.8 Si 288.2
F 703.7, 712.8 SiCl 287.1
Ga 417.2 SiF 440.1, 777.0
H 486.1, 656.5