'''The etch process:'''
'''The etch process:'''<br>
As an example, let's take the etching of silicon by fluorine in one of the dry etchers. The fluorine is supplied to the system as SF<sub>6</sub> gas that is fed to the process chamber using mass flow controllers. Driven by the RF generators (both coil and platen) the plasma will decompose the gas in a series of dissociation and ionisation reactions to form fluorine radicals F<sup>*</sup>. In the areas on the wafer that are not covered by a mask, the exposed silicon atoms will be attacked aggressively by the fluorine radical to form volatile SiF. As such, the SiF will desorp from the wafer surface and eventually get pumped away.
As an example, let's take the etching of silicon by fluorine in one of the dry etchers. The fluorine is supplied to the system as SF<sub>6</sub> gas that is fed to the process chamber using mass flow controllers. Driven by the RF generators (both coil and platen) the plasma will decompose the gas in a series of dissociation and ionisation reactions to form fluorine radicals F<sup>*</sup>. In the areas on the wafer that are not covered by a mask, the exposed silicon atoms will be attacked aggressively by the fluorine radical to form volatile SiF. As such, the SiF will desorp from the wafer surface and eventually get pumped away.


'''The plasma:'''
'''The plasma:'''<br>
The plasma emits light as the gas constituents are continuously exited
The plasma emits light as the gas constituents are continuously exited



Revision as of 15:36, 26 November 2020

Optical endpoint detection on the dry etch tools at DTU Nanolab

Several dry etch tools at DTU Nanolab are equipped with an endpoint detection system. Out of those systems only one is not of the type optical endpoint detection. The instruments are:

  • ICP Metal Etch
  • III-V ICP
  • Pegasus 1
  • Pegasus 4

The section below describes the principle behind the optical endpoint detection system.

Optical Emission Spectroscopy

The etch process:
As an example, let's take the etching of silicon by fluorine in one of the dry etchers. The fluorine is supplied to the system as SF6 gas that is fed to the process chamber using mass flow controllers. Driven by the RF generators (both coil and platen) the plasma will decompose the gas in a series of dissociation and ionisation reactions to form fluorine radicals F*. In the areas on the wafer that are not covered by a mask, the exposed silicon atoms will be attacked aggressively by the fluorine radical to form volatile SiF. As such, the SiF will desorp from the wafer surface and eventually get pumped away.

The plasma:
The plasma emits light as the gas constituents are continuously exited

fdgsdfg

Monitored species Wavelength (nm) Monitored species Wavelength (nm)
Al 308.2, 309.3, 396.1 In 325.6
AlCl 261.4 N 674.0
As 235.0 N2 315.9, 337.1
C2 516.5 NO 247.9, 288.5, 289.3, 303.5, 304.3, 319.8, 320.7, 337.7, 338.6
CF2 251.9 O 777.2, 844.7
Cl 741.4 OH 281.1, 306.4, 308.9
CN 289.8, 304.2, 387.0 S 469.5
CO 292.5, 302.8, 313.8, 325.3, 482.5, 483.5, 519.8 Si 288.2
F 703.7, 712.8 SiCl 287.1
Ga 417.2 SiF 440.1, 777.0
H 486.1, 656.5