Jump to content

Specific Process Knowledge/Etch/DRIE-Pegasus/Isotropic/mediumiso1: Difference between revisions

From LabAdviser
Jmli (talk | contribs)
No edit summary
Jmli (talk | contribs)
No edit summary
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/DRIE-Pegasus/Isotropic/mediumiso1 click here]'''
<!--Checked for updates on 30/7-2018 - ok/jmli -->
<!--Checked for updates on 30/7-2018 - ok/jmli -->
<!--Checked for updates on 2/10-2020 - ok/jmli -->
<!--Checked for updates on 2/10-2020 - ok/jmli -->

Revision as of 09:34, 5 October 2020

Feedback to this page: click here

Process runs
Date Substrate Information Process Information SEM Images
Wafer info Mask Material/ Exposed area Tool / Operator Conditioning Recipe Wafer ID Comments
9/4-2014 4" travka05 wafer 1.5 µm AZ Si / 5 % Pegasus/jmli 5 minute TDESC clean + MU runs jml/isotropic/mediumiso1 2:00 minutes S003961

6/6-2016 6" travka35 wafer 1.5 µm AZ Si / 35 % Pegasus/jmli standard/danchip/mediumiso1 2:00 minutes S006534

6/6-2016 6" travka35 wafer 1.5 µm AZ Si / 35 % Pegasus/jmli standard/danchip/mediumiso1 4:00 minutes S006535