Below is a summary of information compiled Spring 2020 when we considered depositing Mg at Nanolab. | Below is a summary of information compiled Spring 2020 when we considered depositing Mg at Nanolab. | ||
== | ==Mg advice spring 2020== | ||
Input collected by Rebecca (reet) | Input collected by Rebecca (reet) | ||
| Line 13: | Line 13: | ||
*At Penn State they used a cryo pump with Mg e-beam evaporation for many experiments (at least 2 students and several papers) apparently without issues with the pump. | *At Penn State they used a cryo pump with Mg e-beam evaporation for many experiments (at least 2 students and several papers) apparently without issues with the pump. | ||
===Input from Barbara Shaw, Penn State University | ===Input from Barbara Shaw, Penn State University === | ||
E-beam evaporation of Mg | |||
*Best w dedicated system for Mg, the Nanofab lab at Penn State doesn’t allow Mg. | *Best w dedicated system for Mg, the Nanofab lab at Penn State doesn’t allow Mg. | ||
*Recommend major cleaning prior to Mg, predeposit a bunch of Mg. Major clean afterwards and predeposit next material too. Sounds like their system hasn’t been used for other stuff after Mg, so no experience with that. | *Recommend major cleaning prior to Mg, predeposit a bunch of Mg. Major clean afterwards and predeposit next material too. Sounds like their system hasn’t been used for other stuff after Mg, so no experience with that. | ||
*They had no issues w Mg and their cryo pump as far as she knows. | *They had no issues w Mg and their cryo pump as far as she knows. | ||
===Michael Störmer, Helmholtz-Zentrum Geesthacht Zentrum für Material- und Küstenforschung | ===Michael Störmer, Helmholtz-Zentrum Geesthacht Zentrum für Material- und Küstenforschung === | ||
Sputter deposition and also cathode arc and ion beam sputtering of Mg | |||
*Mg challenging, different to other metals. Oxidizes easily - think about the environment for the prepared films. | *Mg challenging, different to other metals. Oxidizes easily - think about the environment for the prepared films. | ||
*On cross-contamination: You see the effect of Mg on the base pressure, as you do for Ti coatings, Michael doesn’t think it’s a long-lasting effect. But - don’t underestimate cleanliness. | *On cross-contamination: You see the effect of Mg on the base pressure, as you do for Ti coatings, Michael doesn’t think it’s a long-lasting effect. But - don’t underestimate cleanliness. | ||
*It is possible to contact them and visit their lab. They have a lot of expertise on Mg. | *It is possible to contact them and visit their lab. They have a lot of expertise on Mg. | ||
===Diederik Depla, Ghent University | ===Diederik Depla, Ghent University=== | ||
Sputtering including HiPIMS of Mg | |||
*Mainly used their setup for Mg, haven’t checked cross-contamination. | *Mainly used their setup for Mg, haven’t checked cross-contamination. | ||
*Believes that Mg on vent will turn into MgO (stable/low-sputter-yield) which should not be a big problem in terms of contamination | *Believes that Mg on vent will turn into MgO (stable/low-sputter-yield) which should not be a big problem in terms of contamination | ||
*They used a turbo/rotary vane pump, no specific reason. | *They used a turbo/rotary vane pump, no specific reason. | ||
*Mg sputters easily, easy to handle targets compared to Ca and Li (sic!). During non-reactive sputtering, MgO will form on target but Mg sputters so fast it’s not a big issue. | *Mg sputters easily, easy to handle targets compared to Ca and Li (sic!). During non-reactive sputtering, MgO will form on target but Mg sputters so fast it’s not a big issue. | ||
Revision as of 11:37, 4 August 2020
Deposition of Magnesium
Magnesium is a relatively volatile metal and we have never deposited it here at Nanolab. Because of its high vapor pressure it is not well suited for deposition in multi-user systems as it will easily re-evaporate from the chamber surfaces and contaminate the films of subsequent users. We are also concerned about deposition of Mg in a chamber with a cryo pump as a very volatile metal may clog the pump.
If you wish to deposit magnesium, please explore options with collaborators at other institutions.
Below is a summary of information compiled Spring 2020 when we considered depositing Mg at Nanolab.
Mg advice spring 2020
Input collected by Rebecca (reet)
- None of the groups we wrote to have mentioned that they have experience with using the chamber for something else after using it for Mg.
- At Penn State they used a cryo pump with Mg e-beam evaporation for many experiments (at least 2 students and several papers) apparently without issues with the pump.
Input from Barbara Shaw, Penn State University
E-beam evaporation of Mg
- Best w dedicated system for Mg, the Nanofab lab at Penn State doesn’t allow Mg.
- Recommend major cleaning prior to Mg, predeposit a bunch of Mg. Major clean afterwards and predeposit next material too. Sounds like their system hasn’t been used for other stuff after Mg, so no experience with that.
- They had no issues w Mg and their cryo pump as far as she knows.
Michael Störmer, Helmholtz-Zentrum Geesthacht Zentrum für Material- und Küstenforschung
Sputter deposition and also cathode arc and ion beam sputtering of Mg
- Mg challenging, different to other metals. Oxidizes easily - think about the environment for the prepared films.
- On cross-contamination: You see the effect of Mg on the base pressure, as you do for Ti coatings, Michael doesn’t think it’s a long-lasting effect. But - don’t underestimate cleanliness.
- It is possible to contact them and visit their lab. They have a lot of expertise on Mg.
Diederik Depla, Ghent University
Sputtering including HiPIMS of Mg
- Mainly used their setup for Mg, haven’t checked cross-contamination.
- Believes that Mg on vent will turn into MgO (stable/low-sputter-yield) which should not be a big problem in terms of contamination
- They used a turbo/rotary vane pump, no specific reason.
- Mg sputters easily, easy to handle targets compared to Ca and Li (sic!). During non-reactive sputtering, MgO will form on target but Mg sputters so fast it’s not a big issue.