|10Å to 1 µm*
|10 Å to 1 µm *
|10Å to 1 µm*
|10 Å to 1 µm *
|10Å to 2000 Å
|10 Å to 2000 Å
|10Å to 5000 Å
|10 Å to 5000 Å **
|10Å to 5000 Å
|10 Å to 5000 Å **
|~20 µm to ~1000 µm
|~20 µm to ~1000 µm
|-
|-
Line 149: Line 149:
*Thicknesses above 2000 Å  requires special permission
*Thicknesses above 2000 Å  requires special permission
|
|
|May use high-strength magnet for deposition
|
|May use high-strength magnet for deposition
*May use high-strength magnet for deposition.
*Thicknesses above 2000 Å require special permission
|
*May use high-strength magnet for deposition
*Thicknesses above 2000 Å require special permission
|Sample must be compatible with plating bath (pH = 3,65 and T = 52°C). Seed metal necessary.
|Sample must be compatible with plating bath (pH = 3,65 and T = 52°C). Seed metal necessary.
|-
|-
Line 156: Line 160:
|}
|}


'''*''' ''To deposit layers thicker than 600 nanometers permission is required from metal@nanolab.dtu.dk to ensure enough material is present in the machine''
'''*''' ''To deposit layers thicker than 600 nm permission is required from metal@nanolab.dtu.dk to ensure enough material is present in the machine''
'''**''' ''To deposit layers thicker than 200 nm permission is required from metal@nanolab.dtu.dk to ensure enough material is present in the machine''

Revision as of 10:39, 21 April 2020

Feedback to this page: click here

Nickel deposition

Nickel can be deposited by e-beam evaporation or electroplating. In the chart below you can compare the different deposition equipment.


E-beam evaporation (Temescal) E-beam evaporation (Wordentec) E-beam evaporation (Physimeca) Sputter deposition (Lesker) Sputter deposition (Cluster-based sputter system) Electroplating (Electroplating-Ni)
General description E-beam deposition of Nickel E-beam deposition of Nickel E-beam deposition of Nickel Sputter deposition of Nickel Sputter deposition of Nickel Electroplating of Nickel
Pre-clean Ar ion bombardment RF Ar clean RF Ar clean RF Ar clean None
Layer thickness 10 Å to 1 µm * 10 Å to 1 µm * 10 Å to 2000 Å 10 Å to 5000 Å ** 10 Å to 5000 Å ** ~20 µm to ~1000 µm
Deposition rate 2Å/s to 10Å/s 10Å/s to 15Å/s 1 to 10Å/s Depends on process parameters. About 1 Å/s Depends on process parameters. About 10 Å/s to 250 Å/s
Batch size
  • Up to 4x6" wafers
  • Up to 3x8" wafers (ask for holder)
  • Many smaller pieces
  • 24x2" wafers or
  • 6x4" wafers or
  • 6x6" wafers
  • 1x 2" wafer or
  • 1x 4" wafers or
  • Several smaller pieces
  • Pieces or
  • 1x4" wafer or
  • 1x6" wafer
  • Up to 10x4" or 6" wafers
  • Many smaller pieces
  • 1x2" wafer or
  • 1x4" wafer or
  • 1x6" wafer
Allowed materials
  • Silicon
  • Silicon oxide
  • Silicon nitride
  • Silicon (oxy)nitride
  • Photoresist
  • PMMA
  • Mylar
  • SU-8
  • Silicon
  • Silicon oxide
  • Silicon (oxy)nitride
  • Photoresist
  • PMMA
  • Mylar
  • SU-8
  • Metals
  • Silicon
  • Silicon oxide
  • Silicon (oxy)nitride
  • Photoresist
  • Metals
  • Almost any that do not outgas if you plan to use substrate heating. Check the cross-contamination sheets in Labmanager.

Base materials:

  • Silicon
  • Polymers with Tg > 75°C
  • Metals (bulk)
  • Cross-linked or hard baked resists supported by one of the above mentioned materials

Seed metals:

  • NiV (75 - 100 nm recommended)
  • Ti (~5 nm) + Au (75-100 nm recommended)
  • Cr (~5 nm) + Au (75-100 nm recommended)
  • TiW
  • Cr
Comment Thicknesses above 2000 Å requires special permission
  • May use high-strength magnet for deposition.
  • Thicknesses above 2000 Å require special permission
  • May use high-strength magnet for deposition
  • Thicknesses above 2000 Å require special permission
Sample must be compatible with plating bath (pH = 3,65 and T = 52°C). Seed metal necessary.

* To deposit layers thicker than 600 nm permission is required from metal@nanolab.dtu.dk to ensure enough material is present in the machine ** To deposit layers thicker than 200 nm permission is required from metal@nanolab.dtu.dk to ensure enough material is present in the machine