Specific Process Knowledge/Lithography/Descum: Difference between revisions
Appearance
No edit summary |
|||
| Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/Descum click here]''' | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/Descum click here]''' | ||
<!-- Replace "http://labadviser.danchip.dtu.dk/..." with the link to the Labadviser page--> | <!-- Replace "http://labadviser.danchip.dtu.dk/..." with the link to the Labadviser page--> | ||
[[Category: Equipment |Lithography descum]] | |||
[[Category: Lithography|Descum]] | |||
==Descum results== | ==Descum results== | ||
Revision as of 10:34, 22 December 2020
Feedback to this page: click here
Descum results
Plasma asher 1

Descum of AZ5214E resist on 50mm silicon wafer. Wafer was placed horisontally in chamber on a 100 mm carier wafer.
Note: Plasma asher was cold before use
| ||||||||||||||||||||||||||||||||||||||||||||||||||
Conny Hjort & Jesper Hanberg September 2019
Plasma asher 2

Descum of AZ Mir 701 resist on 100mm silicon wafer. Five wafers were placed vertically in chamber.
Experiment parameters:
|
recipe 1
|

recipe 2
|
We can observe linear dependance of etched material on time after etching 7 minutes and more (recipe 2).
Jitka Urbánková & Jesper Hanberg
December 2019