Elemental composition analysis
With a unique set of electronic states, each element has its own "finger-print" in the XPS spectrum. The electronic states in the atoms are occupied by electrons with a specific binding energy. In the spectrum above, the dominant peaks of carbon, oxygen and silicon are labelled. More peaks are seen in this socalled survey spectrum but they are all associated to these three elements. All elements have peaks within the wide energy range (usually 0 - 1350 eV binding energy) of the survey spectrum - hence any element that is present in the sample within its detection limit (roughly 1 % depending on element and acquisition setup) will show up in the survey spectrum as peaks of intensities that are determined by the respective concentrations. As such, survey spectra are used to determined what elements are present in the sample.
For each element identified in the survey spectrum, one typically runs a spectrum at the dominant peak. These spectra have a much narrower energy ranges and therefore much smaller energy steps - this enables us to achieve much better energy resolution and hence to see the finer details of each element. These spectra, called high resolution spectra, contain the chemical information that is the strong selling point of the XPS technique.
Table with approximate binding energies
The table below has been adapted from [1].
nyetg
| Element | K 1s | L1 2s | L2 2p1/2 | L3 2p3/2 | M1 3s | M2 3p1/2 | M3 3p3/2 | M4 3d3/2 | M5 3d5/2 | N1 4s | N2 4p1/2 | N3 4p3/2 | N5 4d5/2 | N6 4f5/2 | N7 4f7/2 | O1 5s | O2 5p1/2 | O3 5p3/2 | O4 5d3/2 | O5 5d5/2 | P1 6s | P2 6p1/2 | P3 6p3/2 |
| 37 Rb | 15200 | 2065 | 1864 | 1804 | 326,7 | 248,7 | 239,1 | 113 | 112 | 30,5 | 16,3 | 15,3 | |||||||||||
| 38 Sr | 16105 | 2216 | 2007 | 1940 | 358,7 | 280,3 | 270 | 136 | 134,2 | 38,9 | 21,3 | 20,1 | |||||||||||
| 39 Y | 17038 | 2373 | 2156 | 2080 | 392 | 310,6 | 298,8 | 157,7 | 155,8 | 43,8 | 24,4 | 23,1 | |||||||||||
| 40 Zr | 17998 | 2532 | 2307 | 2223 | 430,3 | 343,5 | 329,8 | 181,1 | 178,8 | 50,6 | 28,5 | 27,1 | |||||||||||
| 41 Nb | 18986 | 2698 | 2465 | 2371 | 466,6 | 376,1 | 360,6 | 205 | 202,3 | 56,4 | 32,6 | 30,8 | |||||||||||
| 42 Mo | 20000 | 2866 | 2625 | 2520 | 506,3 | 411,6 | 394 | 231,1 | 227,9 | 63,2 | 37,6 | 35,5 | |||||||||||
| 43 Tc | 21044 | 3043 | 2793 | 2677 | 544 | 447,6 | 417,7 | 257,6 | 253,9 | 69,5 | 42,3 | 39,9 | |||||||||||
| 44 Ru | 22117 | 3224 | 2967 | 2838 | 586,1 | 483,5 | 461,4 | 284,2 | 280 | 75 | 46,3 | 43,2 | |||||||||||
| 45 Rh | 23220 | 3412 | 3146 | 3004 | 628,1 | 521,3 | 496,5 | 311,9 | 307,2 | 81,4 | 50,5 | 47,3 | |||||||||||
| 46 Pd | 24350 | 3604 | 3330 | 3173 | 671,6 | 559,9 | 532,3 | 340,5 | 335,2 | 87,1 | 55,7 | 50,9 | |||||||||||
| 47 Ag | 25514 | 3806 | 3524 | 3351 | 719 | 603,8 | 573 | 374 | 368,3 | 97 | 63,7 | 58,3 | |||||||||||
| 48 Cd | 26711 | 4018 | 3727 | 3538 | 772 | 652,6 | 618,4 | 411,9 | 405,2 | 109,8 | 63,9 | 63,9 | 11,7 | 10,7 | |||||||||
| 49 In | 27940 | 4238 | 3938 | 3730 | 827,2 | 703,2 | 665,3 | 451,4 | 443,9 | 122,9 | 73,5 | 73,5 | 17,7 | 16,9 | |||||||||
| 50 Sn | 29200 | 4465 | 4156 | 3929 | 884,7 | 756,5 | 714,6 | 493,2 | 484,9 | 137,1 | 83,6 | 83,6 | 24,9 | 23,9 | |||||||||
| 51 Sb | 30491 | 4698 | 4380 | 4132 | 946 | 812,7 | 766,4 | 537,5 | 528,2 | 153,2 | 95,6 | 95,6 | 33,3 | 32,1 | |||||||||
| 52 Te | 31814 | 4939 | 4612 | 4341 | 1006 | 870,8 | 820 | 583,4 | 573 | 169,4 | 103,3 | 103,3 | 41,9 | 40,4 | |||||||||
| 53 I | 33169 | 5188 | 4852 | 4557 | 1072 | 931 | 875 | 630,8 | 619,3 | 186 | 123 | 123 | 50,6 | 48,9 | |||||||||
| 54 Xe | 34561 | 5453 | 5107 | 4786 | 1148,7 | 1002,1 | 940,6 | 689 | 676,4 | 213,2 | 146,7 | 145,5 | 69,5 | 67,5 | — | — | 23,3 | 13,4 | 12,1 | ||||
| 55 Cs | 35985 | 5714 | 5359 | 5012 | 1211 | 1071 | 1003 | 740,5 | 726,6 | 232,3 | 172,4 | 161,3 | 79,8 | 77,5 | — | — | 22,7 | 14,2 | 12,1 | ||||
| 56 Ba | 37441 | 5989 | 5624 | 5247 | 1293 | 1137 | 1063 | 795,7 | 780,5 | 253,5 | 192 | 178,6 | 92,6 | 89,9 | — | — | 30,3 | 17 | 14,8 | ||||
| 57 La | 38925 | 6266 | 5891 | 5483 | 1362 | 1209 | 1128 | 853 | 836 | 274,7 | 205,8 | 196 | 105,3 | 102,5 | — | — | 34,3 | 19,3 | 16,8 | ||||
| 58 Ce | 40443 | 6549 | 6164 | 5723 | 1436 | 1274 | 1187 | 902,4 | 883,8 | 291 | 223,2 | 206,5 | 109 | — | 0,1 | 0,1 | 37,8 | 19,8 | 17 | ||||
| 59 Pr | 41991 | 6835 | 6440 | 5964 | 1511 | 1337 | 1242 | 948,3 | 928,8 | 304,5 | 236,3 | 217,6 | 115,1 | 115,1 | 2 | 2 | 37,4 | 22,3 | 22,3 | ||||
| 60 Nd | 43569 | 7126 | 6722 | 6208 | 1575 | 1403 | 1297 | 1003,3 | 980,4 | 319,2 | 243,3 | 224,6 | 120,5 | 120,5 | 1,5 | 1,5 | 37,5 | 21,1 | 21,1 | ||||
| 61 Pm | 45184 | 7428 | 7013 | 6459 | 1471 | 1357 | 1052 | 1027 | 242 | 242 | 120 | 120 | — | — | — | — | — | ||||||
| 62 Sm | 46834 | 7737 | 7312 | 6716 | 1723 | 1541 | 1420 | 1110,9 | 1083,4 | 347,2 | 265,6 | 247,4 | 129 | 129 | 5,2 | 5,2 | 37,4 | 21,3 | 21,3 | ||||
| 63 Eu | 48519 | 8052 | 7617 | 6977 | 1800 | 1614 | 1481 | 1158,6 | 1127,5 | 360 | 284 | 257 | 133 | 127,7 | 0 | 0 | 32 | 22 | 22 | ||||
| 64 Gd | 50239 | 8376 | 7930 | 7243 | 1881 | 1688 | 1544 | 1221,9 | 1189,6 | 378,6 | 286 | 271 | — | 142,6 | 8,6 | 8,6 | 36 | 28 | 21 | ||||
| 65 Tb | 51996 | 8708 | 8252 | 7514 | 1968 | 1768 | 1611 | 1276,9 | 1241,1 | 396 | 322,4 | 284,1 | 150,5 | 150,5 | 7,7 | 2,4 | 45,6 | 28,7 | 22,6 | ||||
| 66 Dy | 53789 | 9046 | 8581 | 7790 | 2047 | 1842 | 1676 | 1333 | 1292,6 | 414,2 | 333,5 | 293,2 | 153,6 | 153,6 | 8 | 4,3 | 49,9 | 26,3 | 26,3 | ||||
| 67 Ho | 55618 | 9394 | 8918 | 8071 | 2128 | 1923 | 1741 | 1392 | 1351 | 432,4 | 343,5 | 308,2 | 160 | 160 | 8,6 | 5,2 | 49,3 | 30,8 | 24,1 | ||||
| 68 Er | 57486 | 9751 | 9264 | 8358 | 2207 | 2006 | 1812 | 1453 | 1409 | 449,8 | 366,2 | 320,2 | 167,6 | 167,6 | — | 4,7 | 50,6 | 31,4 | 24,7 | ||||
| 69 Tm | 59390 | 10116 | 9617 | 8648 | 2307 | 2090 | 1885 | 1515 | 1468 | 470,9 | 385,9 | 332,6 | 175,5 | 175,5 | — | 4,6 | 54,7 | 31,8 | 25 | ||||
| 70 Yb | 61332 | 10486 | 9978 | 8944 | 2398 | 2173 | 1950 | 1576 | 1528 | 480,5 | 388,7 | 339,7 | 191,2 | 182,4 | 2,5 | 1,3 | 52 | 30,3 | 24,1 | ||||
| 71 Lu | 63314 | 10870 | 10349 | 9244 | 2491 | 2264 | 2024 | 1639 | 1589 | 506,8 | 412,4 | 359,2 | 206,1 | 196,3 | 8,9 | 7,5 | 57,3 | 33,6 | 26,7 | ||||
| 72 Hf | 65351 | 11271 | 10739 | 9561 | 2601 | 2365 | 2108 | 1716 | 1662 | 538 | 438,2 | 380,7 | 220 | 211,5 | 15,9 | 14,2 | 64,2 | 38 | 29,9 | ||||
| 73 Ta | 67416 | 11682 | 11136 | 9881 | 2708 | 2469 | 2194 | 1793 | 1735 | 563,4 | 463,4 | 400,9 | 237,9 | 226,4 | 23,5 | 21,6 | 69,7 | 42,2 | 32,7 | ||||
| 74 W | 69525 | 12100 | 11544 | 10207 | 2820 | 2575 | 2281 | 1872 | 1809 | 594,1 | 490,4 | 423,6 | 255,9 | 243,5 | 33,6 | 31,4 | 75,6 | 45,3 | 36,8 | ||||
| 75 Re | 71676 | 12527 | 11959 | 10535 | 2932 | 2682 | 2367 | 1949 | 1883 | 625,4 | 518,7 | 446,8 | 273,9 | 260,5 | 42,9 | 40,5 | 83 | 45,6 | 34,6 | ||||
| 76 Os | 73871 | 12968 | 12385 | 10871 | 3049 | 2792 | 2457 | 2031 | 1960 | 658,2 | 549,1 | 470,7 | 293,1 | 278,5 | 53,4 | 50,7 | 84 | 58 | 44,5 | ||||
| 77 Ir | 76111 | 13419 | 12824 | 11215 | 3174 | 2909 | 2551 | 2116 | 2040 | 691,1 | 577,8 | 495,8 | 311,9 | 296,3 | 63,8 | 60,8 | 95,2 | 63 | 48 | ||||
| 78 Pt | 78395 | 13880 | 13273 | 11564 | 3296 | 3027 | 2645 | 2202 | 2122 | 725,4 | 609,1 | 519,4 | 331,6 | 314,6 | 74,5 | 71,2 | 101,7 | 65,3 | 51,7 | ||||
| 79 Au | 80725 | 14353 | 13734 | 11919 | 3425 | 3148 | 2743 | 2291 | 2206 | 762,1 | 642,7 | 546,3 | 353,2 | 335,1 | 87,6 | 84 | 107,2 | 74,2 | 57,2 | ||||
| 80 Hg | 83102 | 14839 | 14209 | 12284 | 3562 | 3279 | 2847 | 2385 | 2295 | 802,2 | 680,2 | 576,6 | 378,2 | 358,8 | 104 | 99,9 | 127 | 83,1 | 64,5 | 9,6 | 7,8 | ||
| 81 Tl | 85530 | 15347 | 14698 | 12658 | 3704 | 3416 | 2957 | 2485 | 2389 | 846,2 | 720,5 | 609,5 | 405,7 | 385 | 122,2 | 117,8 | 136 | 94,6 | 73,5 | 14,7 | 12,5 | ||
| 82 Pb | 88005 | 15861 | 15200 | 13035 | 3851 | 3554 | 3066 | 2586 | 2484 | 891,8 | 761,9 | 643,5 | 434,3 | 412,2 | 141,7 | 136,9 | 147 | 106,4 | 83,3 | 20,7 | 18,1 | ||
| 83 Bi | 90524 | 16388 | 15711 | 13419 | 3999 | 3696 | 3177 | 2688 | 2580 | 939 | 805,2 | 678,8 | 464 | 440,1 | 162,3 | 157 | 159,3 | 119 | 92,6 | 26,9 | 23,8 | ||
| 84 Po | 93105 | 16939 | 16244 | 13814 | 4149 | 3854 | 3302 | 2798 | 2683 | 995 | 851 | 705 | 500 | 473 | 184 | 184 | 177 | 132 | 104 | 31 | 31 | ||
| 85 At | 95730 | 17493 | 16785 | 14214 | 4317 | 4008 | 3426 | 2909 | 2787 | 1042 | 886 | 740 | 533 | 507 | 210 | 210 | 195 | 148 | 115 | 40 | 40 | ||
| 86 Rn | 98404 | 18049 | 17337 | 14619 | 4482 | 4159 | 3538 | 3022 | 2892 | 1097 | 929 | 768 | 567 | 541 | 238 | 238 | 214 | 164 | 127 | 48 | 48 | 26 | |
| 87 Fr | 101137 | 18639 | 17907 | 15031 | 4652 | 4327 | 3663 | 3136 | 3000 | 1153 | 980 | 810 | 603 | 577 | 268 | 268 | 234 | 182 | 140 | 58 | 58 | 34 | 15 |
| 88 Ra | 103922 | 19237 | 18484 | 15444 | 4822 | 4490 | 3792 | 3248 | 3105 | 1208 | 1058 | 879 | 636 | 603 | 299 | 299 | 254 | 200 | 153 | 68 | 68 | 44 | 19 |
| 89 Ac | 106755 | 19840 | 19083 | 15871 | 5002 | 4656 | 3909 | 3370 | 3219 | 1269 | 1080 | 890 | 675 | 639 | 319 | 319 | 272 | 215 | 167 | 80 | 80 | — | — |
| 90 Th | 109651 | 20472 | 19693 | 16300 | 5182 | 4830 | 4046 | 3491 | 3332 | 1330 | 1168 | 966,4 | 712,1 | 675,2 | 342,4 | 333,1 | 290 | 229 | 182 | 92,5 | 85,4 | 41,4 | 24,5 |
| 91 Pa | 112601 | 21105 | 20314 | 16733 | 5367 | 5001 | 4174 | 3611 | 3442 | 1387 | 1224 | 1007 | 743 | 708 | 371 | 360 | 310 | 232 | 232 | 94 | 94 | — | — |
| 92 U | 115606 | 21757 | 20948 | 17166 | 5548 | 5182 | 4303 | 3728 | 3552 | 1439 | 1271 | 1043 | 778,3 | 736,2 | 388,2 | 377,4 | 321 | 257 | 192 | 102,8 | 94,2 | 43,9 | 26,8 |
sf
| Shell | K | L1 | L2 | L3 | M1 | M2 | M3 |
| Orbital | 1s | 2s | 2p1/2 | 2p3/2 | 3s | 3p1/2 | 3p3/2 |
| 1 H | 13,6 | ||||||
| 2 He | 24,6 | ||||||
| 3 Li | 54,7 | ||||||
| 4 Be | 111,5 | ||||||
| 5 B | 188 | ||||||
| 6 C | 284,2 | ||||||
| 7 N | 409,9 | 37,3 | |||||
| 8 O | 543,1 | 41,6 | |||||
| 9 F | 696,7 | ||||||
| 10 Ne | 870,2 | 48,5 | 21,7 | 21,6 | |||
| 11 Na | 1070,8 | 63,5 | 30,65 | 30,81 | |||
| 12 Mg | 1303 | 88,7 | 49,78 | 49,5 | |||
| 13 Al | 1559,6 | 117,8 | 72,95 | 72,55 | |||
| 14 Si | 1839 | 149,7 | 99,82 | 99,42 | |||
| 15 P | 2145,5 | 189 | 136 | 135 | |||
| 16 S | 2472 | 230,9 | 163,6 | 162,5 | |||
| 17 Cl | 2822,4 | 270 | 202 | 200 | |||
| 18 Ar | 3205,9 | 326,3 | 250,6 | 248,4 | 29,3 | 15,9 | 15,7 |
| 19 K | 3608,4 | 378,6 | 297,3 | 294,6 | 34,8 | 18,3 | 18,3 |
| 20 Ca | 4038,5 | 438,4 | 349,7 | 346,2 | 44,3 | 25,4 | 25,4 |
| 21 Sc | 4492 | 498 | 403,6 | 398,7 | 51,1 | 28,3 | 28,3 |
| 22 Ti | 4966 | 560,9 | 460,2 | 453,8 | 58,7 | 32,6 | 32,6 |
| 23 V | 5465 | 626,7 | 519,8 | 512,1 | 66,3 | 37,2 | 37,2 |
| 24 Cr | 5989 | 696 | 583,8 | 574,1 | 74,1 | 42,2 | 42,2 |
| 25 Mn | 6539 | 769,1 | 649,9 | 638,7 | 82,3 | 47,2 | 47,2 |
| 26 Fe | 7112 | 844,6 | 719,9 | 706,8 | 91,3 | 52,7 | 52,7 |
| 27 Co | 7709 | 925,1 | 793,2 | 778,1 | 101 | 58,9 | 59,9 |
| 28 Ni | 8333 | 1008,6 | 870 | 852,7 | 110,8 | 68 | 66,2 |
| 29 Cu | 8979 | 1096,7 | 952,3 | 932,7 | 122,5 | 77,3 | 75,1 |
niooib
| Shell | K | L1 | L2 | L3 | M1 | M2 | M3 | M4 | M5 | N1 | N2 | N3 | N5 | N6 |
| Orbital | 1s | 2s | 2p1/2 | 2p3/2 | 3s | 3p1/2 | 3p3/2 | 3d3/2 | 3d5/2 | 4s | 4p1/2 | 4p3/2 | 4d3/2 | 4d5/2 |
| 30 Zn | 9659 | 1196,2 | 1044,9 | 1021,8 | 139,8 | 91,4 | 88,6 | 10,2 | 10,1 | |||||
| 31 Ga | 10367 | 1299 | 1143,2 | 1116,4 | 159,5 | 103,5 | 100 | 18,7 | 18,7 | |||||
| 32 Ge | 11103 | 1414,6 | 1248,1 | 1217 | 180,1 | 124,9 | 120,8 | 29,8 | 29,2 | |||||
| 33 As | 11867 | 1527 | 1359,1 | 1323,6 | 204,7 | 146,2 | 141,2 | 41,7 | 41,7 | |||||
| 34 Se | 12658 | 1652 | 1474,3 | 1433,9 | 229,6 | 166,5 | 160,7 | 55,5 | 54,6 | |||||
| 35 Br | 13474 | 1782 | 1596 | 1550 | 257 | 189 | 182 | 70 | 69 | |||||
| 36 Kr | 14326 | 1921 | 1730,9 | 1678,4 | 292,8 | 222,2 | 214,4 | 95 | 93,8 | 27,5 | 14,1 | 14,1 | ||
| 37 Rb | 15200 | 2065 | 1864 | 1804 | 326,7 | 248,7 | 239,1 | 113 | 112 | 30,5 | 16,3 | 15,3 | ||
| 38 Sr | 16105 | 2216 | 2007 | 1940 | 358,7 | 280,3 | 270 | 136 | 134,2 | 38,9 | 21,3 | 20,1 | ||
| 39 Y | 17038 | 2373 | 2156 | 2080 | 392 | 310,6 | 298,8 | 157,7 | 155,8 | 43,8 | 24,4 | 23,1 | ||
| 40 Zr | 17998 | 2532 | 2307 | 2223 | 430,3 | 343,5 | 329,8 | 181,1 | 178,8 | 50,6 | 28,5 | 27,1 | ||
| 41 Nb | 18986 | 2698 | 2465 | 2371 | 466,6 | 376,1 | 360,6 | 205 | 202,3 | 56,4 | 32,6 | 30,8 | ||
| 42 Mo | 20000 | 2866 | 2625 | 2520 | 506,3 | 411,6 | 394 | 231,1 | 227,9 | 63,2 | 37,6 | 35,5 | ||
| 43 Tc | 21044 | 3043 | 2793 | 2677 | 544 | 447,6 | 417,7 | 257,6 | 253,9 | 69,5 | 42,3 | 39,9 | ||
| 44 Ru | 22117 | 3224 | 2967 | 2838 | 586,1 | 483,5 | 461,4 | 284,2 | 280 | 75 | 46,3 | 43,2 | ||
| 45 Rh | 23220 | 3412 | 3146 | 3004 | 628,1 | 521,3 | 496,5 | 311,9 | 307,2 | 81,4 | 50,5 | 47,3 | ||
| 46 Pd | 24350 | 3604 | 3330 | 3173 | 671,6 | 559,9 | 532,3 | 340,5 | 335,2 | 87,1 | 55,7 | 50,9 | ||
| 47 Ag | 25514 | 3806 | 3524 | 3351 | 719 | 603,8 | 573 | 374 | 368,3 | 97 | 63,7 | 58,3 | ||
| 48 Cd | 26711 | 4018 | 3727 | 3538 | 772 | 652,6 | 618,4 | 411,9 | 405,2 | 109,8 | 63,9 | 63,9 | 11,7 | 10,7 |
| 49 In | 27940 | 4238 | 3938 | 3730 | 827,2 | 703,2 | 665,3 | 451,4 | 443,9 | 122,9 | 73,5 | 73,5 | 17,7 | 16,9 |
| 50 Sn | 29200 | 4465 | 4156 | 3929 | 884,7 | 756,5 | 714,6 | 493,2 | 484,9 | 137,1 | 83,6 | 83,6 | 24,9 | 23,9 |
| 51 Sb | 30491 | 4698 | 4380 | 4132 | 946 | 812,7 | 766,4 | 537,5 | 528,2 | 153,2 | 95,6 | 95,6 | 33,3 | 32,1 |
| 52 Te | 31814 | 4939 | 4612 | 4341 | 1006 | 870,8 | 820 | 583,4 | 573 | 169,4 | 103,3 | 103,3 | 41,9 | 40,4 |
| 53 I | 33169 | 5188 | 4852 | 4557 | 1072 | 931 | 875 | 630,8 | 619,3 | 186 | 123 | 123 | 50,6 | 48,9 |
her
| Shell | K | L1 | L2 | L3 | M1 | M2 | M3 | M4 | M5 | N1 | N2 | N3 | N5 | N6 | N7 | O1 | O2 | O3 | O4 |
| Orbital | 1s | 2s | 2p1/2 | 2p3/2 | 3s | 3p1/2 | 3p3/2 | 3d3/2 | 3d5/2 | 4s | 4p1/2 | 4p3/2 | 4d3/2 | 4d5/2 | 4f5/2 | 4f7/2 | 5s | 5p1/2 | 5p3/2 |
| 54 Xe | 34561 | 5453 | 5107 | 4786 | 1148,7 | 1002,1 | 940,6 | 689 | 676,4 | 213,2 | 146,7 | 145,5 | 69,5 | 67,5 | — | — | 23,3 | 13,4 | 12,1 |
| 55 Cs | 35985 | 5714 | 5359 | 5012 | 1211 | 1071 | 1003 | 740,5 | 726,6 | 232,3 | 172,4 | 161,3 | 79,8 | 77,5 | — | — | 22,7 | 14,2 | 12,1 |
| 56 Ba | 37441 | 5989 | 5624 | 5247 | 1293 | 1137 | 1063 | 795,7 | 780,5 | 253,5 | 192 | 178,6 | 92,6 | 89,9 | — | — | 30,3 | 17 | 14,8 |
| 57 La | 38925 | 6266 | 5891 | 5483 | 1362 | 1209 | 1128 | 853 | 836 | 274,7 | 205,8 | 196 | 105,3 | 102,5 | — | — | 34,3 | 19,3 | 16,8 |
| 58 Ce | 40443 | 6549 | 6164 | 5723 | 1436 | 1274 | 1187 | 902,4 | 883,8 | 291 | 223,2 | 206,5 | 109 | — | 0,1 | 0,1 | 37,8 | 19,8 | 17 |
| 59 Pr | 41991 | 6835 | 6440 | 5964 | 1511 | 1337 | 1242 | 948,3 | 928,8 | 304,5 | 236,3 | 217,6 | 115,1 | 115,1 | 2 | 2 | 37,4 | 22,3 | 22,3 |
| 60 Nd | 43569 | 7126 | 6722 | 6208 | 1575 | 1403 | 1297 | 1003,3 | 980,4 | 319,2 | 243,3 | 224,6 | 120,5 | 120,5 | 1,5 | 1,5 | 37,5 | 21,1 | 21,1 |
| 61 Pm | 45184 | 7428 | 7013 | 6459 | 1471 | 1357 | 1052 | 1027 | 242 | 242 | 120 | 120 | — | — | — | — | — | ||
| 62 Sm | 46834 | 7737 | 7312 | 6716 | 1723 | 1541 | 1420 | 1110,9 | 1083,4 | 347,2 | 265,6 | 247,4 | 129 | 129 | 5,2 | 5,2 | 37,4 | 21,3 | 21,3 |
| 63 Eu | 48519 | 8052 | 7617 | 6977 | 1800 | 1614 | 1481 | 1158,6 | 1127,5 | 360 | 284 | 257 | 133 | 127,7 | 0 | 0 | 32 | 22 | 22 |
| 64 Gd | 50239 | 8376 | 7930 | 7243 | 1881 | 1688 | 1544 | 1221,9 | 1189,6 | 378,6 | 286 | 271 | — | 142,6 | 8,6 | 8,6 | 36 | 28 | 21 |
| 65 Tb | 51996 | 8708 | 8252 | 7514 | 1968 | 1768 | 1611 | 1276,9 | 1241,1 | 396 | 322,4 | 284,1 | 150,5 | 150,5 | 7,7 | 2,4 | 45,6 | 28,7 | 22,6 |
| 66 Dy | 53789 | 9046 | 8581 | 7790 | 2047 | 1842 | 1676 | 1333 | 1292,6 | 414,2 | 333,5 | 293,2 | 153,6 | 153,6 | 8 | 4,3 | 49,9 | 26,3 | 26,3 |
| 67 Ho | 55618 | 9394 | 8918 | 8071 | 2128 | 1923 | 1741 | 1392 | 1351 | 432,4 | 343,5 | 308,2 | 160 | 160 | 8,6 | 5,2 | 49,3 | 30,8 | 24,1 |
| 68 Er | 57486 | 9751 | 9264 | 8358 | 2207 | 2006 | 1812 | 1453 | 1409 | 449,8 | 366,2 | 320,2 | 167,6 | 167,6 | — | 4,7 | 50,6 | 31,4 | 24,7 |
| 69 Tm | 59390 | 10116 | 9617 | 8648 | 2307 | 2090 | 1885 | 1515 | 1468 | 470,9 | 385,9 | 332,6 | 175,5 | 175,5 | — | 4,6 | 54,7 | 31,8 | 25 |
| 70 Yb | 61332 | 10486 | 9978 | 8944 | 2398 | 2173 | 1950 | 1576 | 1528 | 480,5 | 388,7 | 339,7 | 191,2 | 182,4 | 2,5 | 1,3 | 52 | 30,3 | 24,1 |
| 71 Lu | 63314 | 10870 | 10349 | 9244 | 2491 | 2264 | 2024 | 1639 | 1589 | 506,8 | 412,4 | 359,2 | 206,1 | 196,3 | 8,9 | 7,5 | 57,3 | 33,6 | 26,7 |
| 72 Hf | 65351 | 11271 | 10739 | 9561 | 2601 | 2365 | 2108 | 1716 | 1662 | 538 | 438,2 | 380,7 | 220 | 211,5 | 15,9 | 14,2 | 64,2 | 38 | 29,9 |
| 73 Ta | 67416 | 11682 | 11136 | 9881 | 2708 | 2469 | 2194 | 1793 | 1735 | 563,4 | 463,4 | 400,9 | 237,9 | 226,4 | 23,5 | 21,6 | 69,7 | 42,2 | 32,7 |
| 74 W | 69525 | 12100 | 11544 | 10207 | 2820 | 2575 | 2281 | 1872 | 1809 | 594,1 | 490,4 | 423,6 | 255,9 | 243,5 | 33,6 | 31,4 | 75,6 | 45,3 | 36,8 |
| 75 Re | 71676 | 12527 | 11959 | 10535 | 2932 | 2682 | 2367 | 1949 | 1883 | 625,4 | 518,7 | 446,8 | 273,9 | 260,5 | 42,9 | 40,5 | 83 | 45,6 | 34,6 |
| 76 Os | 73871 | 12968 | 12385 | 10871 | 3049 | 2792 | 2457 | 2031 | 1960 | 658,2 | 549,1 | 470,7 | 293,1 | 278,5 | 53,4 | 50,7 | 84 | 58 | 44,5 |
| 77 Ir | 76111 | 13419 | 12824 | 11215 | 3174 | 2909 | 2551 | 2116 | 2040 | 691,1 | 577,8 | 495,8 | 311,9 | 296,3 | 63,8 | 60,8 | 95,2 | 63 | 48 |
| 78 Pt | 78395 | 13880 | 13273 | 11564 | 3296 | 3027 | 2645 | 2202 | 2122 | 725,4 | 609,1 | 519,4 | 331,6 | 314,6 | 74,5 | 71,2 | 101,7 | 65,3 | 51,7 |
| 79 Au | 80725 | 14353 | 13734 | 11919 | 3425 | 3148 | 2743 | 2291 | 2206 | 762,1 | 642,7 | 546,3 | 353,2 | 335,1 | 87,6 | 84 | 107,2 | 74,2 | 57,2 |
nut
| Shell | K | L1 | L2 | L3 | M1 | M2 | M3 | M4 | M5 | N1 | N2 | N3 | N4 | N5 | N6 | N7 | O1 | O2 | O3 | O4 | O5 | P1 | P2 | P3 |
| Orbital | 1s | 2s | 2p1/2 | 2p3/2 | 3s | 3p1/2 | 3p3/2 | 3d3/2 | 3d5/2 | 4s | 4p1/2 | 4p3/2 | 4d3/2 | 4d5/2 | 4f5/2 | 4f7/2 | 5s | 5p1/2 | 5p3/2 | 5d3/2 | 5d5/2 | 6s | 6p1/2 | 6p3/2 |
| 80 Hg | 83102 | 14839 | 14209 | 12284 | 3562 | 3279 | 2847 | 2385 | 2295 | 802,2 | 680,2 | 576,6 | 378,2 | 358,8 | 104 | 99,9 | 127 | 83,1 | 64,5 | 9,6 | 7,8 | |||
| 81 Tl | 85530 | 15347 | 14698 | 12658 | 3704 | 3416 | 2957 | 2485 | 2389 | 846,2 | 720,5 | 609,5 | 405,7 | 385 | 122,2 | 117,8 | 136 | 94,6 | 73,5 | 14,7 | 12,5 | |||
| 82 Pb | 88005 | 15861 | 15200 | 13035 | 3851 | 3554 | 3066 | 2586 | 2484 | 891,8 | 761,9 | 643,5 | 434,3 | 412,2 | 141,7 | 136,9 | 147 | 106,4 | 83,3 | 20,7 | 18,1 | |||
| 83 Bi | 90524 | 16388 | 15711 | 13419 | 3999 | 3696 | 3177 | 2688 | 2580 | 939 | 805,2 | 678,8 | 464 | 440,1 | 162,3 | 157 | 159,3 | 119 | 92,6 | 26,9 | 23,8 | |||
| 84 Po | 93105 | 16939 | 16244 | 13814 | 4149 | 3854 | 3302 | 2798 | 2683 | 995 | 851 | 705 | 500 | 473 | 184 | 184 | 177 | 132 | 104 | 31 | 31 | |||
| 85 At | 95730 | 17493 | 16785 | 14214 | 4317 | 4008 | 3426 | 2909 | 2787 | 1042 | 886 | 740 | 533 | 507 | 210 | 210 | 195 | 148 | 115 | 40 | 40 | |||
| 86 Rn | 98404 | 18049 | 17337 | 14619 | 4482 | 4159 | 3538 | 3022 | 2892 | 1097 | 929 | 768 | 567 | 541 | 238 | 238 | 214 | 164 | 127 | 48 | 48 | 26 | ||
| 87 Fr | 101137 | 18639 | 17907 | 15031 | 4652 | 4327 | 3663 | 3136 | 3000 | 1153 | 980 | 810 | 603 | 577 | 268 | 268 | 234 | 182 | 140 | 58 | 58 | 34 | 15 | 15 |
| 88 Ra | 103922 | 19237 | 18484 | 15444 | 4822 | 4490 | 3792 | 3248 | 3105 | 1208 | 1058 | 879 | 636 | 603 | 299 | 299 | 254 | 200 | 153 | 68 | 68 | 44 | 19 | 19 |
| 89 Ac | 106755 | 19840 | 19083 | 15871 | 5002 | 4656 | 3909 | 3370 | 3219 | 1269 | 1080 | 890 | 675 | 639 | 319 | 319 | 272 | 215 | 167 | 80 | 80 | — | — | - |
| 90 Th | 109651 | 20472 | 19693 | 16300 | 5182 | 4830 | 4046 | 3491 | 3332 | 1330 | 1168 | 966,4 | 712,1 | 675,2 | 342,4 | 333,1 | 290 | 229 | 182 | 92,5 | 85,4 | 41,4 | 24,5 | 16,6 |
| 91 Pa | 112601 | 21105 | 20314 | 16733 | 5367 | 5001 | 4174 | 3611 | 3442 | 1387 | 1224 | 1007 | 743 | 708 | 371 | 360 | 310 | 232 | 232 | 94 | 94 | — | — | - |
| 92 U | 115606 | 21757 | 20948 | 17166 | 5548 | 5182 | 4303 | 3728 | 3552 | 1439 | 1271 | 1043 | 778,3 | 736,2 | 388,2 | 377,4 | 321 | 257 | 192 | 102,8 | 94,2 | 43,9 | 26,8 | 16,8 |