|'''Ashing time (min)'''|| 1 ||2 ||3 ||4 ||5 ||6 ||7 ||8 ||10 ||12 ||15 ||20
|'''Ashing time (min)'''|| 1 ||2 ||3 ||4 ||5 ||6 ||7 ||8 ||10 ||12 ||15 ||20
|-  
|-  
|'''Etched Thickness (nm)'''||8,1 ||9,4 ||16,8 ||55,2 ||44,0 ||47,5 ||42,5 ||55,1416 ||85,3 ||122,4 ||184,8 ||305,9
|'''Etched Thickness (nm)'''||8,1 ||9,4 ||16,8 ||55,2 ||44,0 ||47,5 ||42,5 ||55,1 ||85,3 ||122,4 ||184,8 ||305,9
|-  
|-  
|'''Initial temperature (°C)'''||22 ||21 ||21 ||22 ||22 ||22 ||21 ||21 ||20 ||21 ||21 ||22
|'''Initial temperature (°C)'''||22 ||21 ||21 ||22 ||22 ||22 ||21 ||21 ||20 ||21 ||21 ||22

Revision as of 15:14, 12 December 2019

Feedback to this page: click here

Descum results

Plasma asher 1

Descum results plasma asher 1


Descum of AZ5214E resist on 50mm silicon wafer. Wafer was placed horisontally in chamber on a 100 mm carier wafer.

Note: Plasma asher was cold before use

Settings Etched Thickness (nm)
ashing time (min)
Recipe O2 flow N2 flow Power 1 2 5 7 10 10
1 70 70 150 14,2 16,3 47,6 123,2 854,3 862,1
2 500 0 200 8,1 32,9 271,1 495,6 446,2

Conny Hjort & Jesper Hanberg September 2019



Plasma asher 2

Descum results plasma asher 2 - recipe 1

Descum of AZ Mir 701 resist on 100mm silicon wafer. Five wafers were placed vertically in chamber.

Experiment parameters:

O2 flow N2 flow Power
recipe 1 100 100 150
recipe 2 500 0 200


recipe 1

Ashing time (min) 1 2 3 4 6 7 8 9 10 12 14 15 20
Etched Thickness (nm) 8,7 5,1 12,5 6,2 31,8 86,0 25,7 46,8 38,3 49,7 59,4 140,1 360,7
Initial temperature (°C) 28 21 31 21 22 28 25 24 21 24 24 22 22


recipe 2

Ashing time (min) 1 2 3 4 5 6 7 8 10 12 15 20
Etched Thickness (nm) 8,1 9,4 16,8 55,2 44,0 47,5 42,5 55,1 85,3 122,4 184,8 305,9
Initial temperature (°C) 22 21 21 22 22 22 21 21 20 21 21 22