Slow etch of silicon nitride with resist as masking material - on 6" carrier wafer with recess
This recipe can be used for slow etching of silicon nitride with resist as masking material. Here are some test results presented. The same recipe is being used for SiO2, see the result for that here
Parameter | A slow etch with carrier |
---|---|
Coil Power [W] | 200 |
Platen Power [W] | 25 |
Platen temperature [oC] | 0 |
CF4 flow [sccm] | 20 |
H2 flow [sccm] | 10 |
Pressure [mTorr] | 3 |
Results | Test on wafer with 20% load, by Izzet Yildiz @Nanotech | Test by BGHE @nanolab |
---|---|---|
Etch rate of LPCVD nitride | 60-65 nm/min (20% etch load) (Feb. 2014) | |
Selectivity to resist [SiN : AZ resist] | 1:0.75 | |
Wafer uniformity (100mm) | ? | |
Profile [o] | ? | |
Wafer uniformity map (click on the image to view a larger image) | not measured | |
SEM profile images | Not measured | |
Etch rate in Barc | ~50 nm/min (Date: 2014-09-09) | |
Etch rate in KRF resist | ~40 nm/min (Date: 2014-09-09) |