[[image:Descum Results aug 2019.png|right|frame| Descum results]]


Descum of AZ5214E resist on 50mm silicon wafer. Wafer was placed horisontally in chamber on a 100 mm carier wafer.
Descum of AZ5214E resist on 50mm silicon wafer. Wafer was placed horisontally in chamber on a 100 mm carier wafer.

Revision as of 12:31, 30 August 2019

Descum results

Plasma asher 1

Descum results

Descum of AZ5214E resist on 50mm silicon wafer. Wafer was placed horisontally in chamber on a 100 mm carier wafer.

Note: Plasma asher was cold before use

Settings Etched Thickness (nm)
ashing time (min)
Recipe O2 flow N2 flow Power 1 2 5 7 10 10
1 70 70 150 14,2 16,3 47,6 123,2 854,3 862,1