Specific Process Knowledge/Lithography/DUVStepperLithography: Difference between revisions
No edit summary |
|||
Line 3: | Line 3: | ||
[[Image:stepper_image_1.jpg|300x300px|right|thumb|DUV Stepper is placed in F-3]] | [[Image:stepper_image_1.jpg|300x300px|right|thumb|DUV Stepper is placed in F-3]] | ||
'''Feedback to this section''': '''[mailto:labadviser@ | '''Feedback to this section''': '''[mailto:labadviser@anolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/DUVStepperLithography#DUV_Stepper_FPA-3000EX4_from_Canon click here]''' | ||
The deep-UV stepper FPA-3000EX4 from Canon is an advanced exposure system designed for mass-production of 6 and 8 inch wafers/ devices having a throughput of up to 90 wafers per hour. The largest applicable thickness of the wafers/ devices is 1,2 mm. Also 4" wafers/ devices can be processed with some restrictions concerning throughput, resolution, uniformity and maximum allowed wafer thickness. The system is equipped with a KrF Excimer laser from Cymer (wavelength 248 nm). Its projection lens’ NA is variable over a range between 0,4 and 0,6. Additionally, the partial coherence factor (σ) of the illumination system can be adjusted and different off-axis illumination modes can be selected. | The deep-UV stepper FPA-3000EX4 from Canon is an advanced exposure system designed for mass-production of 6 and 8 inch wafers/ devices having a throughput of up to 90 wafers per hour. The largest applicable thickness of the wafers/ devices is 1,2 mm. Also 4" wafers/ devices can be processed with some restrictions concerning throughput, resolution, uniformity and maximum allowed wafer thickness. The system is equipped with a KrF Excimer laser from Cymer (wavelength 248 nm). Its projection lens’ NA is variable over a range between 0,4 and 0,6. Additionally, the partial coherence factor (σ) of the illumination system can be adjusted and different off-axis illumination modes can be selected. | ||
Line 11: | Line 11: | ||
'''The user manual(s), quality control procedure(s) and results and contact information can be found in LabManager:''' | '''The user manual(s), quality control procedure(s) and results and contact information can be found in LabManager:''' | ||
Equipment info in [http://labmanager | Equipment info in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=273 LabManager] | ||
== Process information == | == Process information == | ||
Line 90: | Line 90: | ||
[[Image:Gamma_2M.jpg|300x300px|right|thumb|The SÜSS Spinner-Stepper is placed in F-3]] | [[Image:Gamma_2M.jpg|300x300px|right|thumb|The SÜSS Spinner-Stepper is placed in F-3]] | ||
'''Feedback to this section''': '''[mailto:labadviser@ | '''Feedback to this section''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/DUVStepperLithography#S.C3.9CSS_Spinner-Stepper click here]''' | ||
This spinner is dedicated for spinning DUV resists. The spinner is fully automatic and can run up to 25 substrates in a batch 4", 6", and 8" size (8" requires tool change). The machine is equipped with the 3 resist lines (DUV42S-6, KRF M230Y, and KRF M35G), an automatic syringe system and a solvent line for cleaning and back-side rinse. | This spinner is dedicated for spinning DUV resists. The spinner is fully automatic and can run up to 25 substrates in a batch 4", 6", and 8" size (8" requires tool change). The machine is equipped with the 3 resist lines (DUV42S-6, KRF M230Y, and KRF M35G), an automatic syringe system and a solvent line for cleaning and back-side rinse. | ||
'''The user manual, and contact information can be found in LabManager:''' | '''The user manual, and contact information can be found in LabManager:''' | ||
Equipment info in [http://labmanager | Equipment info in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=279 LabManager] | ||
==Process information== | ==Process information== | ||
Line 193: | Line 193: | ||
[[Image:SUSS_DEV.JPG|300x300px|right|thumb|The Developer-TMAH-Stepper is placed in F-3]] | [[Image:SUSS_DEV.JPG|300x300px|right|thumb|The Developer-TMAH-Stepper is placed in F-3]] | ||
'''Feedback to this section''': '''[mailto:labadviser@ | '''Feedback to this section''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/DUVStepperLithography#Developer_TMAH_Stepper click here]''' | ||
This developer is dedicated for development of DUV resists. The developer is fully automatic and can run up to 25 substrates in a batch 4", 6", and 8" size (8" requires tool change). The machine is equipped with 1 developer line, in our case 2,38% TMAH in water (AZ 726 MIF), 1 topside rinse line with water, 1 backside rinse line with water and 1 N2 line for drying. | This developer is dedicated for development of DUV resists. The developer is fully automatic and can run up to 25 substrates in a batch 4", 6", and 8" size (8" requires tool change). The machine is equipped with 1 developer line, in our case 2,38% TMAH in water (AZ 726 MIF), 1 topside rinse line with water, 1 backside rinse line with water and 1 N2 line for drying. | ||
'''The user manual and contact information can be found in LabManager:''' | '''The user manual and contact information can be found in LabManager:''' | ||
Equipment info in [http://labmanager | Equipment info in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=328 LabManager] | ||
<br clear="all" /> | <br clear="all" /> | ||
==Process information== | ==Process information== | ||
[[Image:140 250 nm tilt22 (1).jpg|350x350px|right|thumb|The SEM picture of | [[Image:140 250 nm tilt22 (1).jpg|350x350px|right|thumb|The SEM picture of 250 nm pillars and lines. Exposure dose is 140 J/m2.]] | ||
The development process will be performed by the customer together with the Photolith group of Danchip. In case you would like to do DUV lithography please contact Lithography team, who will consult you and run your wafers together with you. | The development process will be performed by the customer together with the Photolith group of Danchip. In case you would like to do DUV lithography please contact Lithography team, who will consult you and run your wafers together with you. | ||
Here you can find a [[media:250nm_ines_and_pillars_after_developing_i_60sec.pdf| chart]] demonstrating a dependence between | Here you can find a [[media:250nm_ines_and_pillars_after_developing_i_60sec.pdf| chart]] demonstrating a dependence between 250 nm line width/pillars diameter and exposure dose. | ||
===Standard processes=== | ===Standard processes=== |
Revision as of 18:05, 25 November 2019
DUV Stepper
Feedback to this section: click here
The deep-UV stepper FPA-3000EX4 from Canon is an advanced exposure system designed for mass-production of 6 and 8 inch wafers/ devices having a throughput of up to 90 wafers per hour. The largest applicable thickness of the wafers/ devices is 1,2 mm. Also 4" wafers/ devices can be processed with some restrictions concerning throughput, resolution, uniformity and maximum allowed wafer thickness. The system is equipped with a KrF Excimer laser from Cymer (wavelength 248 nm). Its projection lens’ NA is variable over a range between 0,4 and 0,6. Additionally, the partial coherence factor (σ) of the illumination system can be adjusted and different off-axis illumination modes can be selected.
The critical dimension (CD) of patterns that can be realized is specified at around 250nm for arbitrary formed patterns in the standard illumination mode (NA=0,6; σ =0,65). However, the best achievable resolution is different for each pattern type, pattern shape and pitch. So linewidths down to 160 nm could be achieved for geometrically simple patterns or pattern arrays (single and multiple line or pin-hole structures).
The user manual(s), quality control procedure(s) and results and contact information can be found in LabManager:
Equipment info in LabManager
Process information
Purpose |
Exposure system designed for mass/production of devices with linewidth down to 250nm | ||
---|---|---|---|
Specifications | Magnification |
1:5 | |
Projection lens Numerical Aperture |
0,4 - 0,60 | ||
Illumination system's σ |
0,2 - 0,75 (standard illumination mode: σ = 0,65) | ||
Exposure source |
KrF laser | ||
Wavelength |
248nm | ||
Illumination intensity |
2800 W/m2 | ||
Illumination uniformity |
1,2% | ||
Maximum printed field size |
22 x 26 mm (maximum on wafer) | ||
Alignment accuracy |
3 sigma = 50 nm | ||
Substrates | Substrate size |
| |
Allowed materials |
| ||
Batch |
1 - 25 |
SÜSS Spinner-Stepper
Feedback to this section: click here
This spinner is dedicated for spinning DUV resists. The spinner is fully automatic and can run up to 25 substrates in a batch 4", 6", and 8" size (8" requires tool change). The machine is equipped with the 3 resist lines (DUV42S-6, KRF M230Y, and KRF M35G), an automatic syringe system and a solvent line for cleaning and back-side rinse.
The user manual, and contact information can be found in LabManager: Equipment info in LabManager
Process information
The spinning process will be performed by the customer together with the Photolith group of Danchip. In case you would like to do DUV lithography please contact Lithography team, who will consult you and run your wafers together with you.
Information about resist can be found here:
- Bottom Anti Reflection Coating (BARC) DUV 42S-6 Datasheet DUV42S-6.
- Positive DUV resist for spin coating in 600-300nm thickness range KRF M230Y.
- Positive DUV resist for spin coating in 1600-800nm thickness range KRF M35G.
- Negative DUV resist for spin coating in 1400-800nm or diluted with EC Solvent in 1:1 in 400-200nm thickness range UVN2300-0.8.
Standard processes
BARC DUV42S-6 coating sequences:
- (1201) DCH 150mm BARC 65nm Dispense 3ml@1000rpm; spin-off 30s@4700rpm; softbake 60s@175°C
- (1202) DCH 100mm BARC 65nm Dispense 1.6ml@1000rpm; spin-off 30s@3000rpm; softbake 60s@175°C
KRF M230Y coating sequences:
- (1301) DCH 150mm M230Y 360nm Dispense 3ml@1000rpm; spin-off 30s@2500rpm; softbake 90s@130°C
- (1302) DCH 100mm M230Y 360nm Dispense 1ml@1000rpm; spin-off 30s@2500rpm; softbake 90s@130°C
KRF M35G coating sequences:
- (1401) DCH 150mm M35G 750nm Dispense 3ml@1000rpm; spin-off 60s@5000rpm; softbake 90s@130°C
- (1402) DCH 100mm M35G 750nm Dispense 1ml@1000rpm; spin-off 60s@5000rpm; softbake 90s@130°C
- (1403) DCH 150mm M35G 1000nm Dispense 3ml@1000rpm; spin-off 60s@2630rpm; softbake 90s@130°C
- (1404) DCH 100mm M35G 1000nm Dispense 1ml@1000rpm; spin-off 60s@26300rpm; softbake 90s@130°C
- (1405) DCH 150mm M35G 1400nm Dispense 3ml@1000rpm; spin-off 60s@1310rpm; softbake 90s@130°C
- (1406) DCH 100mm M35G 1400nm Dispense 1ml@1000rpm; spin-off 60s@1310rpm; softbake 90s@130°C
Purpose |
| ||
---|---|---|---|
Resist |
| ||
Performance | Coating thickness |
| |
Process parameters | Spin speed |
10 - 5000 rpm | |
Spin acceleration |
100 - 10000 rpm/s | ||
Hotplate temperature |
| ||
Substrates | Substrate size |
| |
Allowed materials |
| ||
Batch |
1 - 25 |
Developer TMAH Stepper
Feedback to this section: click here
This developer is dedicated for development of DUV resists. The developer is fully automatic and can run up to 25 substrates in a batch 4", 6", and 8" size (8" requires tool change). The machine is equipped with 1 developer line, in our case 2,38% TMAH in water (AZ 726 MIF), 1 topside rinse line with water, 1 backside rinse line with water and 1 N2 line for drying.
The user manual and contact information can be found in LabManager: Equipment info in LabManager
Process information
The development process will be performed by the customer together with the Photolith group of Danchip. In case you would like to do DUV lithography please contact Lithography team, who will consult you and run your wafers together with you.
Here you can find a chart demonstrating a dependence between 250 nm line width/pillars diameter and exposure dose.
Standard processes
Post-exposure bake sequences:
- (1000) DCH PEB 130C 60s 60s baking at 130°C; 20s cooling
- (1001) DCH PEB 130C 90s 90s baking at 130°C; 20s cooling
Development sequences:
- (1004) DCH DEV 60s 60s single puddle development
Combined PEB and development sequences:
- (1002) DCH PEB_60s and DEV_60s 60s baking at 130°C followed by 60s single puddle development
- (1003) DCH PEB_90s and DEV_60s 90s baking at 130°C followed by 60s single puddle development
The standard developer process consists of:
- pre-wetting with water (2.5s @ 1000rpm)
- developer dispense (2.5s @ 40rpm, corresponding to ~9ml)
- development (60s @ 0rpm)
- water rinse with BSR (5s @ 3000rpm)
- nitrogen drying (7s @ 4000rpm)
and has a cycle time of ~2 minutes
Purpose |
Development of DUV resist: KRF M230Y and KRF M35G | ||
---|---|---|---|
Developer |
2,38% water based TMAH | ||
Process parameters | Spin speed |
10 - 5000 rpm | |
Spin acceleration |
100 - 10000 rpm/s | ||
Hotplate temperature |
130°C for post exposure baking | ||
Substrates | Substrate size |
| |
Allowed materials |
| ||
Batch |
1 - 25 |