Jump to content

Specific Process Knowledge/Lithography/ZEP520A: Difference between revisions

From LabAdviser
Lgpe (talk | contribs)
No edit summary
Jmli (talk | contribs)
No edit summary
Line 1: Line 1:




This is a standard positive resist from ZEON. The resist is very expensive; DTU Danchip has thus stopped buying this resist.  
This is a standard positive resist from ZEON. The resist is very expensive; DTU Nanolab has thus stopped buying this resist.  
Use CSAR instead.
Use CSAR instead.


Contact lithography@danchip.dtu.dk if you wish to use this resist.
Contact lithography@nanolab.dtu.dk if you wish to use this resist.


== Spin Curves ==
== Spin Curves ==
Line 19: Line 19:
|-
|-
|-style="background:Black; color:White"
|-style="background:Black; color:White"
!colspan="7"|ZEON ZEP520A1:1 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 23-04-2014. Resist was mixed 13-01-2014, i.e. approximatley 3 months old.
!colspan="7"|ZEON ZEP520A1:1 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 23-04-2014. Resist was mixed 13-01-2014, i.e. approximately 3 months old.
|-
|-


Line 64: Line 64:
|-
|-
|-style="background:red; color:White"
|-style="background:red; color:White"
!colspan="7"|ZEON ZEP520A1:1 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 21-05-2014. Resist was mixed 15-05-2014, i.e. approximatley 6 days old.
!colspan="7"|ZEON ZEP520A1:1 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 21-05-2014. Resist was mixed 15-05-2014, i.e. approximately 6 days old.
|-
|-


Line 124: Line 124:
|-
|-
|-style="background:green; color:White"
|-style="background:green; color:White"
!colspan="7"|ZEON ZEP520A1:2 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 21-05-2014. Resist was mixed 15-05-2014, i.e. approximatley 6 days old.
!colspan="7"|ZEON ZEP520A1:2 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 21-05-2014. Resist was mixed 15-05-2014, i.e. approximately 6 days old.
|-
|-



Revision as of 20:34, 25 November 2019


This is a standard positive resist from ZEON. The resist is very expensive; DTU Nanolab has thus stopped buying this resist. Use CSAR instead.

Contact lithography@nanolab.dtu.dk if you wish to use this resist.

Spin Curves


The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on a Si wafer with native oxide. The measurements are performed at one incidence angle (70 degrees) only. 9 points on each 4" wafer has been measured; the standard deviation thus represents the homogeinity of the film on the 4" wafers.

ZEON ZEP520A1:1 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 23-04-2014. Resist was mixed 13-01-2014, i.e. approximately 3 months old.
Spin Speed [rpm] Acceleration [1/s2] Thickness [nm] St Dev
3000 4000 111.29 0.65
4000 4000 95.17 2.16
5000 4000 87.23 0.81


ZEON ZEP520A1:1 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 21-05-2014. Resist was mixed 15-05-2014, i.e. approximately 6 days old.
Spin Speed [rpm] Acceleration [1/s2] Thickness [nm] St Dev
2000 4000 141.03 1.02
3000 4000 115.96 0.98
4000 4000 100.56 0.80
5000 4000 91.01 0.38
6000 4000 84.85 0.37


ZEON ZEP520A1:2 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 21-05-2014. Resist was mixed 15-05-2014, i.e. approximately 6 days old.
Spin Speed [rpm] Acceleration [1/s2] Thickness [nm] St Dev
2000 4000 79.12 1.74
3000 4000 64.30 0.34
4000 4000 55.50 0.48
5000 4000 50.53 0.62
6000 4000 46.34 1.01