Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300/Etch slow: Difference between revisions
Appearance
No edit summary |
|||
| Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@ | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/IBE⁄IBSD_Ionfab_300/Etch_slow click here]''' | ||
=Etch slow (this was tested in 2012 by ''bghe@nanolab'')= | =Etch slow (this was tested in 2012 by ''bghe@nanolab'')= | ||
Revision as of 13:56, 18 August 2021
Feedback to this page: click here
Etch slow (this was tested in 2012 by bghe@nanolab)
This process development was done to find an etch recipe that is so gentle that the resist masking material can be removed with acetone + ultrasound within hopefully 10min. This is important when a metal is to be etched as this cannot withstand plasma ashing (to remove reist mask) after the etch.
| Parameter | Si etch test1 | Si etch test2 | Si etch test3 |
|---|---|---|---|
| Important note | This recipe must only be run for 5 min, otherwise the beam acc. current will incrase above 20 | ||
| Neutalizer current [mA] | 450 | 250 | 450 |
| RF Power [W] | 1200 | 1000 | 1200 |
| Beam current [mA] | 400 | 200 | 400 |
| Beam voltage [V] | 400 | 200 | 400 |
| Beam accelerator voltage | 400 | 200 | 400 |
| Ar flow to neutralizer [sccm] | 6.0 | 6.0 | 6.0 |
| Ar flow to beam [sccm] | 6.0 | 6.0 | 6.0 |
| Rotation speed [rpm] | 20 | 20 | 20 |
| Stage angle [degrees] | 10 | 10 | 10 |
| Platen temp. [dg. Celcius] | 15 | 15 | 15 |
| He cooling pressure [mTorr] | 37.5 | 37.5 | 37.5 |
| Etch material | Si | Si | Si |
| Results | vvv | vvv | vvv |
| Etch time [min] | 40 | 40 | 7:15 |
| Etch rate in Si [nm/min] | 19.7 | 3.58 | 19.3 |
| Total time in Acetone + ultrasound [min] | 17 | 10 | 20 |
| Was the resist completely removed after acetone + ultrasound? | no | yes | yes (almost) |