| Line 63: |
Line 63: |
| !Deposition rate | | !Deposition rate |
| | | | | |
| *3.0-3.5nm/min (reactive DC sputtering) | | *3.0-3.5 nm/min (reactive sputtering) |
| | | | | |
| *3 - 5 nm/min (RF sputtering) | | *3-5 nm/min (RF sputtering) |
| *0.3 - 0.5nm/min | | *0.3 - 0.5 nm/min |
| | | | | |
| * 1 - 2 Å/s | | * 1 - 2 Å/s |
Revision as of 14:09, 13 August 2018
Feedback to this page: click here
Deposition of Titanium Oxide
Titanium oxide can be deposited either by a sputter technique or by use of ALD (atomic layer deposition). At the moment the only system where we have a target for Titanium oxide is IBE/IBSD Ionfab300. The target is Ti. During the sputter deposition oxygen is added to the chamber resulting in Titanium oxide on the sample.
Comparison of the methods for deposition of Titanium Oxide
|
|
Sputter technique using IBE/IBSD Ionfab300
|
Sputter System Lesker
|
III-V Dielectric evaporator
|
ALD Picosun 200
|
| Generel description
|
- TiO2 created from a Ti sputter target. By adding oxygen during the deposition TiO2 is created.
|
- Reactive DC sputtering of Ti target in Ar/O2 (10% O2) plasma.
- RF sputtering of TiO2 target
|
- E-beam evaporation of TiO2
|
- ALD (atomic layer deposition) of TiO2
|
| Stoichiometry
|
- Can probably be varied (sputter target: Ti, O2 added during deposition)
|
|
|
- Temperature dependent - Anatase or amorphous TiO2
|
| Film Thickness
|
|
|
|
|
| Deposition rate
|
- 3.0-3.5 nm/min (reactive sputtering)
|
- 3-5 nm/min (RF sputtering)
- 0.3 - 0.5 nm/min
|
|
- 0.06 nm/min - 0.40 nm/min (very recipe and temperature dependent)
|
| Step coverage
|
|
|
|
- Very good. Covers sample everywhere (but long purge time needed for very high aspect ratio structures)
|
| Process Temperature
|
- Expected to be below 100oC
|
- Done at RT. There is a possibility to run at higher temperatures
|
- Sample temperature can be set to 20-250 oC
|
- 120oC - 150oC: Amorphous TiO2
- 300oC - 350oC: Anatase TiO2
|
| More info on TiO2
|
|
|
|
ALD1:
ALD2:
|
| Substrate size
|
- 1 50mm wafer
- 1 100mm wafer
- 1 150mm wafer
- 1 200mm wafer
- Smaller pieces can be mounted with capton tape
|
- several small samples
- several 50 mm wafers (Ø150mm carrier)
- 1x 100 mm wafers
- 1x 150 mm wafers
|
- 1x 2" wafer or
- several smaller samples
|
ALD1:
- 1-5 100 mm wafers
- 1-5 150 mm wafers
- 1 200 mm wafer
- Several smaller samples
ALD2:
- 1 100 mm wafer
- 1 150 mm wafer
- 1 200 mm wafer
- Several smaller samples
|
| Allowed materials
|
- Almost any materials
- not Pb and very poisonous materials
|
- Almost any materials
- Pb and poisonous materials only after special agreement
|
|
- Silicon
- Silicon oxide, silicon nitride
- Quartz/fused silica
- Metals - Use a dedicated carrier wafer
- III-V materials - Use dedicated carrier wafer
- Polymers - Depending on the melting point/deposition temperature, use dedicated carrier wafer. Ask for permission
|