Jump to content

Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano142: Difference between revisions

From LabAdviser
Jmli (talk | contribs)
No edit summary
Jmli (talk | contribs)
No edit summary
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/DRIE-Pegasus/nanoetch/nano142 click here]'''
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/DRIE-Pegasus/nanoetch/nano142 click here]'''
<!--Checked for updates on 30/7-2018 - ok/jmli -->
<!--Checked for updates on 30/7-2018 - ok/jmli -->
 
<!--Checked for updates on 5/10-2020 - ok/jmli -->
== The nano1.42 recipe ==
== The nano1.42 recipe ==



Revision as of 09:26, 5 October 2020

Feedback to this page: click here

The nano1.42 recipe

Recipe nano1.42
Recipe Gas C4F8 75 sccm, SF6 38 sccm
Pressure 4 mTorr, Strike 3 secs @ 15 mTorr
Power 800 W CP, 40 W PP
Temperature -20 degs
Hardware 100 mm Spacers
Time 120 secs
Conditions Run ID 2017
Conditioning Sequence: Oxygen clean, MU tests, processes, no oxygen between runs
Mask 211 nm zep etched down to 82 nm



Nominal trench line width ' 30 60 90 120 150 Average Std. dev.
Etch rates nm/min 148 158 164 167 166 160 8
Sidewall angle degs 90 90 90 90 90 90 0
CD loss nm/edge 7 -7 -7 -28 -28 -13 15
CD loss foot nm/edge 12 5 6 -15 -1 1 10
Bowing -1 1 -2 -5 -7 -3 3
Bottom curvature -46 -30 -29 -31 -27 -32 8
zep nm/min 65