Specific Process Knowledge/Etch/DRIE-Pegasus/processA: Difference between revisions
| Line 639: | Line 639: | ||
|- | |- | ||
| Trench width (µm)||||5,1||6,7||9,3||11,4||13,7||18,6||29,0||44,5||54,4||80,5||106,7||156,9||207,4||310,1 | | Trench width (µm)||||5,1||6,7||9,3||11,4||13,7||18,6||29,0||44,5||54,4||80,5||106,7||156,9||207,4||310,1 | ||
|- | |||
|} | |||
|} | |||
= Standard Process A 110 cycles = | |||
Post process images: | |||
[[file:C01549.01-A.jpg |200px|frameless|C01549.01 ]] | |||
[[file:C01549.02-A.jpg |200px|frameless|C01549.02 ]] | |||
[[file:C01549.03.jpg |200px|frameless|C01549.03 ]] | |||
[[file:C01549.04-A.jpg |200px|frameless|C01549.04 ]] | |||
[[file:C01549.04-B.jpg |200px|frameless|C01549.04 ]] | |||
{| border="2" cellpadding="0" cellspacing="0" style="text-align:center;" | |||
|+ '''Travkatesting2: Process A run for 110 cycles on travka 5, 10, 20, 35 masks''' | |||
|- | |||
! width="30" rowspan="2" | Date | |||
! width="40" rowspan="2"| Substrate Information | |||
! width="50" rowspan="2"| Process Information | |||
! colspan="15"| SEM images of trenches | |||
! rowspan="2" | Numbers | |||
|- | |||
! 2 µm | |||
! 3 µm | |||
! 4 µm | |||
! 6 µm | |||
! 8 µm | |||
! 10 µm | |||
! 15 µm | |||
! 25 µm | |||
! 40 µm | |||
! 50 µm | |||
! 75 µm | |||
! 100 µm | |||
! 150 µm | |||
! 200 µm | |||
! 300 µm | |||
|- | |||
| January 2013 | |||
| Travka05, 600 nm oxide, '''5% open''' | |||
| Process A 110 cycles or 20:10 minutes, '''C01549.01''' | |||
| [[file:C01549.01 002mu 0129.jpg |75px|frameless ]] | |||
| [[file:C01549.01 004-3mu 0128.jpg |75px|frameless ]] | |||
| [[file:C01549.01 004-3mu 0128.jpg |75px|frameless ]] | |||
| [[file:C01549.01 008-6mu 0127.jpg |75px|frameless ]] | |||
| [[file:C01549.01 008-6mu 0127.jpg |75px|frameless ]] | |||
| [[file:C01549.01 010mu 0126.jpg |75px|frameless ]] | |||
| [[file:C01549.01 015mu 0125.jpg |75px|frameless ]] | |||
| [[file:C01549.01 025mu 0124.jpg |75px|frameless ]] | |||
| [[file:C01549.01 040mu 0123.jpg |75px|frameless ]] | |||
| [[file:C01549.01 050mu 0122.jpg |75px|frameless ]] | |||
| [[file:C01549.01 075mu 0121.jpg |75px|frameless ]] | |||
| [[file:C01549.01 100mu 0120.jpg |75px|frameless ]] | |||
| [[file:C01549.01 150mu 0119.jpg |75px|frameless ]] | |||
| [[file:C01549.01 200mu 0118.jpg |75px|frameless ]] | |||
| [[file:C01549.01 300mu 0117.jpg |75px|frameless ]] | |||
| | |||
{| {{table}} | |||
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)''' | |||
| align="center" style="background:#f0f0f0;"|'''2''' | |||
| align="center" style="background:#f0f0f0;"|'''3''' | |||
| align="center" style="background:#f0f0f0;"|'''4''' | |||
| align="center" style="background:#f0f0f0;"|'''6''' | |||
| align="center" style="background:#f0f0f0;"|'''8''' | |||
| align="center" style="background:#f0f0f0;"|'''10''' | |||
| align="center" style="background:#f0f0f0;"|'''15''' | |||
| align="center" style="background:#f0f0f0;"|'''25''' | |||
| align="center" style="background:#f0f0f0;"|'''40''' | |||
| align="center" style="background:#f0f0f0;"|'''50''' | |||
| align="center" style="background:#f0f0f0;"|'''75''' | |||
| align="center" style="background:#f0f0f0;"|'''100''' | |||
| align="center" style="background:#f0f0f0;"|'''150''' | |||
| align="center" style="background:#f0f0f0;"|'''200''' | |||
| align="center" style="background:#f0f0f0;"|'''300''' | |||
|- | |||
| Etched depth (µm)||175||195||209||229||247||260||289||330||370||393||428||454||488||507||523 | |||
|- | |||
| Av. ER (µm/min)||8,7||9,7||10,4||11,3||12,3||12,9||14,4||16,3||18,3||19,5||21,2||22,5||24,2||25,2||25,9 | |||
|- | |||
| Av. Scllp hght (nm)||1591||1772||1902||2079||2247||2359||2631||2997||3364||3569||3888||4124||4434||4614||4751 | |||
|- | |||
| Sdwall bowing (%)||0,12||0,20||0,30||0,35||0,32||0,35||0,40||0,30||0,41||0,24||0,33||0,32||0,47||0,71||0,00 | |||
|- | |||
| Sdwall angle (degs)||89,6||89,9||89,9||90,1||90,2||90,3||90,7||90,9||91,1||91,4||91,5||91,5||91,2||91,6||91,7 | |||
|- | |||
| Trench width (µm)||8,5||9,5||10,8||13,2||16,0||18,4||22,6||33,0||48,0||57,5||82,7||106,8||159,0||207,0||306,8 | |||
|- | |||
|} | |||
|- | |||
| January 2013 | |||
| Travka10, 600 nm oxide, '''10% open''' | |||
| Process A 110 cycles or 20:10 minutes, '''C01549.02''' | |||
| [[file:C01549.02 002mu 0085.jpg |75px|frameless ]] | |||
| [[file:C01549.02 003mu 0084.jpg |75px|frameless ]] | |||
| [[file:C01549.02 004mu 0083.jpg |75px|frameless ]] | |||
| [[file:C01549.02 006mu 0082.jpg |75px|frameless ]] | |||
| [[file:C01549.02 008mu 0081.jpg |75px|frameless ]] | |||
| [[file:C01549.02 010mu 0080.jpg |75px|frameless ]] | |||
| [[file:C01549.02 015mu 0079.jpg |75px|frameless ]] | |||
| [[file:C01549.02 025mu 0078.jpg |75px|frameless ]] | |||
| [[file:C01549.02 040mu 0077.jpg |75px|frameless ]] | |||
| [[file:C01549.02 050mu 0076.jpg |75px|frameless ]] | |||
| [[file:C01549.02 075mu 0075.jpg |75px|frameless ]] | |||
| [[file:C01549.02 100mu 0074.jpg |75px|frameless ]] | |||
| [[file:C01549.02 150mu 0073.jpg |75px|frameless ]] | |||
| [[file:C01549.02 200mu 0072.jpg |75px|frameless ]] | |||
| [[file:C01549.02 300mu 0071.jpg |75px|frameless ]] | |||
| | |||
{| {{table}} | |||
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)''' | |||
| align="center" style="background:#f0f0f0;"|'''2''' | |||
| align="center" style="background:#f0f0f0;"|'''3''' | |||
| align="center" style="background:#f0f0f0;"|'''4''' | |||
| align="center" style="background:#f0f0f0;"|'''6''' | |||
| align="center" style="background:#f0f0f0;"|'''8''' | |||
| align="center" style="background:#f0f0f0;"|'''10''' | |||
| align="center" style="background:#f0f0f0;"|'''15''' | |||
| align="center" style="background:#f0f0f0;"|'''25''' | |||
| align="center" style="background:#f0f0f0;"|'''40''' | |||
| align="center" style="background:#f0f0f0;"|'''50''' | |||
| align="center" style="background:#f0f0f0;"|'''75''' | |||
| align="center" style="background:#f0f0f0;"|'''100''' | |||
| align="center" style="background:#f0f0f0;"|'''150''' | |||
| align="center" style="background:#f0f0f0;"|'''200''' | |||
| align="center" style="background:#f0f0f0;"|'''300''' | |||
|- | |||
| Etched depth (µm)||164||179||190||209||224||238||263||300||337||358||388||404||438||452||469 | |||
|- | |||
| Av. ER (µm/min)||8,1||8,9||9,4||10,4||11,1||11,8||13,1||14,9||16,7||17,7||19,2||20,0||21,7||22,4||23,2 | |||
|- | |||
| Av. Scllp hght (nm)||1489||1626||1730||1899||2034||2163||2395||2724||3063||3251||3526||3671||3978||4110||4262 | |||
|- | |||
| Sdwall bowing (%)||0,20||0,41||0,46||0,57||0,74||0,62||0,68||0,75||0,58||0,99||0,54||0,49||0,72||0,51||0,77 | |||
|- | |||
| Sdwall angle (degs)||89,7||90,0||89,9||90,1||90,2||90,3||90,8||91,2||91,5||91,3||92,0||92,2||92,6||92,8||93,6 | |||
|- | |||
| Trench width (µm)||7,9||8,7||10,4||12,6||16,1||18,1||22,8||33,5||49,3||58,1||83,1||108,6||157,0||207,1||301,3 | |||
|- | |||
|} | |||
|- | |||
| January 2013 | |||
| Travka20, 600 nm oxide, '''20% open''' | |||
| Process A 110 cycles or 20:10 minutes, '''C01549.03''' | |||
| [[file:C01549.03 002mu 0087.jpg |75px|frameless ]] | |||
| [[file:C01549.03 003mu 0088.jpg |75px|frameless ]] | |||
| [[file:C01549.03 004mu 0089.jpg |75px|frameless ]] | |||
| [[file:C01549.03 006mu 0090.jpg |75px|frameless ]] | |||
| [[file:C01549.03 008mu 0091.jpg |75px|frameless ]] | |||
| [[file:C01549.03 010mu 0092.jpg |75px|frameless ]] | |||
| [[file:C01549.03 015mu 0093.jpg |75px|frameless ]] | |||
| [[file:C01549.03 025mu 0094.jpg |75px|frameless ]] | |||
| [[file:C01549.03 040mu 0095.jpg |75px|frameless ]] | |||
| [[file:C01549.03 050mu 0096.jpg |75px|frameless ]] | |||
| [[file:C01549.03 075mu 0097.jpg |75px|frameless ]] | |||
| [[file:C01549.03 100mu 0098.jpg |75px|frameless ]] | |||
| [[file:C01549.03 150mu 0099.jpg |75px|frameless ]] | |||
| [[file:C01549.03 200mu 0100.jpg |75px|frameless ]] | |||
| [[file:C01549.03 300mu 0101.jpg |75px|frameless ]] | |||
| | |||
{| {{table}} | |||
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)''' | |||
| align="center" style="background:#f0f0f0;"|'''2''' | |||
| align="center" style="background:#f0f0f0;"|'''3''' | |||
| align="center" style="background:#f0f0f0;"|'''4''' | |||
| align="center" style="background:#f0f0f0;"|'''6''' | |||
| align="center" style="background:#f0f0f0;"|'''8''' | |||
| align="center" style="background:#f0f0f0;"|'''10''' | |||
| align="center" style="background:#f0f0f0;"|'''15''' | |||
| align="center" style="background:#f0f0f0;"|'''25''' | |||
| align="center" style="background:#f0f0f0;"|'''40''' | |||
| align="center" style="background:#f0f0f0;"|'''50''' | |||
| align="center" style="background:#f0f0f0;"|'''75''' | |||
| align="center" style="background:#f0f0f0;"|'''100''' | |||
| align="center" style="background:#f0f0f0;"|'''150''' | |||
| align="center" style="background:#f0f0f0;"|'''200''' | |||
| align="center" style="background:#f0f0f0;"|'''300''' | |||
|- | |||
| Etched depth (µm)||142||153||164||181||195||206||228||258||287||303||326||342||366||380||392 | |||
|- | |||
| Av. ER (µm/min)||7,0||7,6||8,1||9,0||9,7||10,2||11,3||12,8||14,2||15,0||16,2||17,0||18,2||18,8||19,4 | |||
|- | |||
| Av. Scllp hght (nm)||1288||1390||1493||1647||1775||1877||2073||2342||2612||2754||2967||3108||3331||3451||3561 | |||
|- | |||
| Sdwall bowing (%)||0,54||0,77||1,08||0,83||1,06||0,91||0,95||1,07||0,88||0,75||0,95||0,05||0,83||0,73||0,46 | |||
|- | |||
| Sdwall angle (degs)||89,6||89,6||89,8||90,2||90,3||90,6||90,9||91,5||91,6||91,8||92,3||93,3||92,5||92,9||93,0 | |||
|- | |||
| Trench width (µm)||7,2||8,7||9,9||12,4||14,7||16,9||22,8||31,1||48,4||58,0||81,9||108,6||160,4||209,9||311,1 | |||
|- | |||
|} | |||
|- | |||
| January 2013 | |||
| Travka35, 600 nm oxide, '''35% open''' | |||
| Process A 110 cycles or 20:10 minutes, '''C01549.04''' | |||
| [[file:C01549.04 003mu 0115.jpg |75px|frameless ]] | |||
| [[file:C01549.04 003mu 0116.jpg |75px|frameless ]] | |||
| [[file:C01549.04 004mu 0114.jpg |75px|frameless ]] | |||
| [[file:C01549.04 006mu 0113.jpg |75px|frameless ]] | |||
| [[file:C01549.04 008mu 0112.jpg |75px|frameless ]] | |||
| [[file:C01549.04 010mu 0111.jpg |75px|frameless ]] | |||
| [[file:C01549.04 015mu 0110.jpg |75px|frameless ]] | |||
| [[file:C01549.04 025mu 0109.jpg |75px|frameless ]] | |||
| [[file:C01549.04 040mu 0108.jpg |75px|frameless ]] | |||
| [[file:C01549.04 050mu 0107.jpg |75px|frameless ]] | |||
| [[file:C01549.04 075mu 0106.jpg |75px|frameless ]] | |||
| [[file:C01549.04 100mu 0105.jpg |75px|frameless ]] | |||
| [[file:C01549.04 150mu 0104.jpg |75px|frameless ]] | |||
| [[file:C01549.04 200mu 0103.jpg |75px|frameless ]] | |||
| [[file:C01549.04 300mu 0102.jpg |75px|frameless ]] | |||
| | |||
{| {{table}} | |||
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)''' | |||
| align="center" style="background:#f0f0f0;"|'''2''' | |||
| align="center" style="background:#f0f0f0;"|'''3''' | |||
| align="center" style="background:#f0f0f0;"|'''4''' | |||
| align="center" style="background:#f0f0f0;"|'''6''' | |||
| align="center" style="background:#f0f0f0;"|'''8''' | |||
| align="center" style="background:#f0f0f0;"|'''10''' | |||
| align="center" style="background:#f0f0f0;"|'''15''' | |||
| align="center" style="background:#f0f0f0;"|'''25''' | |||
| align="center" style="background:#f0f0f0;"|'''40''' | |||
| align="center" style="background:#f0f0f0;"|'''50''' | |||
| align="center" style="background:#f0f0f0;"|'''75''' | |||
| align="center" style="background:#f0f0f0;"|'''100''' | |||
| align="center" style="background:#f0f0f0;"|'''150''' | |||
| align="center" style="background:#f0f0f0;"|'''200''' | |||
| align="center" style="background:#f0f0f0;"|'''300''' | |||
|- | |||
| Etched depth (µm)||||||131||146||155||164||181||205||226||234||254||264||277||284||292 | |||
|- | |||
| Av. ER (µm/min)||||||6,5||7,2||7,7||8,2||9,0||10,2||11,2||11,6||12,6||13,1||13,8||14,1||14,5 | |||
|- | |||
| Av. Scllp hght (nm)||||||1189||1325||1408||1495||1642||1867||2050||2125||2312||2398||2523||2584||2653 | |||
|- | |||
| Sdwall bowing (%)||||||1,35||1,37||1,25||1,28||1,24||1,45||1,30||1,42||1,50||1,38||1,18||0,76||0,81 | |||
|- | |||
| Sdwall angle (degs)||||||89,4||89,6||89,9||90,0||90,3||91,0||91,7||91,9||92,3||92,4||93,0||93,0||93,5 | |||
|- | |||
| Trench width (µm)||||||8,8||11,3||13,5||16,0||21,2||31,1||46,3||56,5||81,2||108,0||157,7||210,0||310,4 | |||
|- | |- | ||
|} | |} | ||
|} | |} | ||
Revision as of 19:34, 1 July 2018
Feedback to this page: click here
Effects on Process A of showerhead change in December 2014
The effects of changing of the showerhead in December 2014 was investigated. Patterned wafers were processed before and after and the profile of the etched features were inspected in SEM. Click on the numbers in the 'Runs' column below to see the profiles.
| Recipe | Name | Temp. | Deposition step | Etch step | Comments | |||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Time | Pres. | C4F8 | SF6 | O2 | Coil | Time | Pres. | C4F8 | SF6 | O2 | Coil | Platen | Showerhead | Runs | Key words | |||
| Process A | Step1 11 cyc | 20 | 4 | 25 | 200 | 0 | 0 | 2000 | 7.0 | 25(1.5s) 90>>150 | 0 | 350(1.5s) 550 | 5 | 2800 | 120>>140(1.5s) 45 | Old | 1 | |
| Step2 44 cyc | 4 | 25 | 200 | 0 | 0 | 2000 | 7.0 | 25(1.5s) 150 | 0 | 350(1.5s) 550 | 5 | 2800 | 140(1.5s) 45 | |||||
| Step1 11 cyc | 20 | 4 | 25 | 200 | 0 | 0 | 2000 | 7.0 | 25(1.5s) 90>>150 | 0 | 350(1.5s) 550 | 5 | 2800 | 120>>140(1.5s) 45 | New | 1 | Profile improved | |
| Step2 44 cyc | 4 | 25 | 200 | 0 | 0 | 2000 | 7.0 | 25(1.5s) 150 | 0 | 350(1.5s) 550 | 5 | 2800 | 140(1.5s) 45 | |||||
Process A acceptance test
Process A is labelled Large trench (80μm wide) 150μm depth. In the acceptance test the process was run on a 150 mm SPTS wafer with 12-13 % etch load.
| Parameter | Specification | Average result |
|---|---|---|
| Etch rate (µm/min) | > 15 | 18.9 |
| Etched depth (µm) | 150 | 189.1 |
| Scallop size (nm) | < 800 | 718 |
| Profile (degs) | 91 +/- 1 | 91.1 |
| Selectivity to AZ photoresist | > 150 | 310 |
| Undercut (µm) | <1.5 | 0.84 |
| Uniformity (%) | < 3.5 | 3.0 |
| Repeatability (%) | <4 | 0.43 |
| Process A parameters | ||||
|---|---|---|---|---|
| Step 1 | Step 2 | |||
| Parameter | Etch | Dep | Etch | Dep |
| Gas flow (sccm) | SF6 350 (1.5 s) 550 | C4F8 200 | SF6 350 (1.5 s) 550 | C4F8 200 |
| Cycle time (secs) | 7.0 | 4.0 | 7.0 | 4.0 |
| Pressure (mtorr) | 25 (1.5 s) 90 >> 150 | 25 | 25 (1.5 s) 150 | 25 |
| Coil power (W) | 2800 | 2000 | 2800 | 2000 |
| Platen power (W) | 120 >> 140 (1.5) 45 | 0 | 140 (1.5) 45 | 0 |
| Cycles | 11 (keep fixed) | 44 (vary this) | ||
| Common | Temperature 20 degs, HBC 10 torr, Short funnel, with baffle & 5mm spacers | |||
Quality control procedure
| Quality Control (QC) for DRIE-Pegasus | |||||||||||||||||
| |||||||||||||||||
Process A guidelines
Process A is optimized for speed and depending on feature size and etch load it will achieve etch rates up to 25-30 µm/min.
This aggressive etch has a few drawbacks - one of which is the release of energy in the etch process. In general, it is clear that
- The higher the etch rate, the higher rate of released energy.
- The larger an area of silicon is exposed to plasma and hence etched, the higher rate of released energy.
Given its high etch rate, Process A is very sensible to high etch load processes and substrates with reduced cooling efficiency. Therefore, users are generally advised to
- Use Process A with precaution at high etch loads - above some 50%.
- Avoid using Process A on bonded wafers, in particular if the etch load is more than 5-10%. The bonding reduces the heat conduction across the wafer interface so the top wafer will immediately heat up and cause the mask to erode and the bonding polymer to melt.
If you have a bonded sandwich of wafers with very poor heat conduction (typically caused by intermediate polymer layers thicker than a few microns) you are advised to use other etch processes, maybe the deepetch on the ASE.
Process A performance
The perfomance of Process A has been investigated as a function of feature size and etch load.
Experiment
A number of wafers are patterned with the Travka mask set in AZ photoresist or 600 nm oxide. The wafers are then etched (batch recipe with 5 minute TDESC interstep cleans) using two different durations of process A in the DRIE-Pegasus.
|
|
Results: Optical images
- Optical images of the C01548 batch that is processed 10:05 mins.
-
Wafer C01548.01: 5 % exposed area
-
Wafer C01548.02: 10 % exposed area
-
Wafer C01548.03: 20 % exposed area
-
Wafer C01548.04: 35 % exposed area
-
Wafer C01548.05: 50 % exposed area
- Optical images of the C01549 batch that is processed 20:10 mins.
-
Wafer C01549.01: 5 % exposed area. Some 190 nm of 600 nm oxide remains.
-
Wafer C01549.02: 10 % exposed area. Some 122 nm oxide remains.
-
Wafer C01549.03: 20 % exposed area. In the centre some 90 nm oxide remains.
-
Wafer C01549.04: 35 % exposed area. In the centre some 90 nm oxide remains.
-
Wafer C01549.05: 35 % exposed area (close-up). The oxide has disappeared leaving the Si exposed.
The etching of silicon releases energy. This means that the faster the etch is, the more heat needs to be dissipated. The consequence is the same if a larger percentage of the wafer is etched. Process A is the fastest etch and as seen above, the exposed area plays an important role. As the exposed area increases the oxide mask erosion is more and more pronounced.
If a larger area is to be etched, the cooling must be made more efficient, either by lowering the platen temperature or with increasing the pressure of He on the backside of the wafer. This will be investigated soon.
Results: Etched depths in trenches of different widths
- Graphs
-
Process time 10:05
-
Process time 20:10
Results: SEM images of trench cross sections
Standard Process A 110 cycles
Post process images:
| Date | Substrate Information | Process Information | SEM images of trenches | Numbers | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| 2 µm | 3 µm | 4 µm | 6 µm | 8 µm | 10 µm | 15 µm | 25 µm | 40 µm | 50 µm | 75 µm | 100 µm | 150 µm | 200 µm | 300 µm | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
| January 2013 | Travka05, 600 nm oxide, 5% open | Process A 110 cycles or 20:10 minutes, C01549.01 |
| |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
| January 2013 | Travka10, 600 nm oxide, 10% open | Process A 110 cycles or 20:10 minutes, C01549.02 |
| |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
| January 2013 | Travka20, 600 nm oxide, 20% open | Process A 110 cycles or 20:10 minutes, C01549.03 |
| |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
| January 2013 | Travka35, 600 nm oxide, 35% open | Process A 110 cycles or 20:10 minutes, C01549.04 |
| |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||