Specific Process Knowledge/Thin film deposition/MVD: Difference between revisions

From LabAdviser
Jml (talk | contribs)
Jml (talk | contribs)
Line 37: Line 37:
== The FLAT recipe ==
== The FLAT recipe ==


The FLAT recipe is designed for coating of non-structured wafers. The amount of FDTS is delivered in one cycle (4 injections pf FDTS at 0.400 Torr + 1 injection of water at 18 Torr) and the reaction time is 15 minutes.
The FLAT recipe is designed for coating of non-structured wafers. The amount of FDTS is delivered in one cycle (4 injections of FDTS at 0.400 Torr + 1 injection of water at 18 Torr) and the reaction time is 15 minutes.
{| border="2" cellpadding="2" cellspacing="1"  
{| border="2" cellpadding="2" cellspacing="1"  
|+'''The FLAT recipe'''
|+'''The FLAT recipe'''
Line 86: Line 86:
|-
|-
|}
|}


== The STAMP recipe ==
== The STAMP recipe ==

Revision as of 21:50, 3 April 2008

The Molecular Vapor Deposition Tool

The MVD is located in cleanroom 1

The Applied Microstructures MVD 100 system deposits molecular films on surfaces. These films serve a wide range of purposes ranging from antistiction coatings of nanoimprint lithography stamps to protecting MEMS structures. At Danchip the MVD is essential for nanoimprint lithography.

Processing on the MVD

The MVD coatings are created as self-assembled monolayers on a surface when a molecular vapor of chemials is present.

These chemicals, typically it is flourinated organosilanes, have a teflon-like tail consisting of -(CF2)xCF3 and, in the other end, a reactive group -Si(teflon)Clx. As shown in the figure below, the chlorine atoms react with -OH groups of the surface to form a chemical bond -Si((teflon))-O-Si(surface)- under elimination of HCL. This means that both Si and SiO2 surfaces are coated because of the native oxide on Si surfaces.

The parameters of the MVD process

The most important parameters to control during the MVD process are:

Substrate surface
A O2 plasma is run prior to any process in order to condition the substrate surface. This will also remove any existing MVD coating.
Water content
Water will cause the chemicals to polymerize (bond to each other instead of on the surface) and it is therefore critical to precisely control the water content.
Substrate temperature
The temperature of the substrate is the same as the process chamber and it is kept constant at 35 oC.
Vapor order
There is no active force that injects the chemicals into the process chamber. The driving force is a combination of two factors:
  1. A pressure gradient The vapor pressure of the chemical (when stored at some temperature in the cylinder) compared to the pressure in the chamber.
  2. A temperature gradient The chemical and the line that feeds the process chamber are kept at a higher temperature.

It is critical that the chemicals with the lowest vapor pressure are injected first into the process chamber. If, for instance, water is injected before FDTS, the water will flow into the FTDS expansion volume and cause polymerization, thus forcing a mechanical clean. NOT GOOD!.

The FLAT recipe

The FLAT recipe is designed for coating of non-structured wafers. The amount of FDTS is delivered in one cycle (4 injections of FDTS at 0.400 Torr + 1 injection of water at 18 Torr) and the reaction time is 15 minutes.

The FLAT recipe
O2 plasma Flow 200 sccm
Power 250 Watts
Time 300 seconds
Chemical # 1 (vapor order 1) Name FDTS
Line no. 3
Cycles 4
Pressure 0.500 Torr
Chemical # 2 (vapor order 2) Name Water
Line no. 1
Cycles 1
Pressure 18 Torr
Processing Time 900 seconds
Purge Cycles 5

The STAMP recipe

The STAMP recipe uses the same total amount of FDTS as FLAT but delivers it much slower in order to obtain a much better and conformal coating of fine nanostructures. A cycle with 1 injection of FDTS at 0.400 Torr + 1 injection of water at 6 Torr reacts for 15 minutes. Then the process chamber is evacuated and a new cycle starts.

and the reaction time is 15 minutes.

The STAMP recipe
O2 plasma Flow 200 sccm
Power 250 Watts
Time 300 seconds
Chemical # 1 (vapor order 1) Name FDTS
Line no. 3
Cycles 4
Pressure 0.500 Torr
Chemical # 2 (vapor order 2) Name Water
Line no. 1
Cycles 1
Pressure 18 Torr
Processing Time 900 seconds
Purge Cycles 5