|Recipe name: ''' | |Recipe name: '''no name yet''' (testing recipe) | ||
|- | |- | ||
|Coil Power [W] | |Coil Power [W] | ||
| | |1200 | ||
|- | |- | ||
|Platen Power [W] | |Platen Power [W] | ||
Line 18: | Line 18: | ||
|0 | |0 | ||
|- | |- | ||
| | |BCl3 flow [sccm] | ||
| | |60 | ||
|- | |- | ||
| | |Cl<sub>2</sub> flow [sccm] | ||
|30 | |||
| | |||
|- | |- | ||
|Pressure [mTorr] | |Pressure [mTorr] | ||
Line 38: | Line 35: | ||
|-style="background:DarkGray; color:White" | |-style="background:DarkGray; color:White" | ||
!Material to be etched | !Material to be etched | ||
!Etch rate using | !Etch rate using the above parameters | ||
|- | |- | ||
| | |Al2O3 | ||
| | | | ||
*'''~230nm/min ( | *'''~230nm/min (1/4 wafer on 6" carrier)''' | ||
|- | |- | ||
|} | |} | ||
<br clear="all" /> | <br clear="all" /> |
Revision as of 15:04, 20 January 2017
Feedback to this page: click here
THIS PAGE IS UNDER CONSTRUCTION![Under construction.png](/images/thumb/f/f8/Under_construction.png/200px-Under_construction.png.jpeg)
Parameter | Recipe name: no name yet (testing recipe) |
---|---|
Coil Power [W] | 1200 |
Platen Power [W] | 200 |
Platen temperature [oC] | 0 |
BCl3 flow [sccm] | 60 |
Cl2 flow [sccm] | 30 |
Pressure [mTorr] | 4 |
Etch rates in different materials using the standard "Silicon oxide etch with resist mask"
Material to be etched | Etch rate using the above parameters |
---|---|
Al2O3 |
|