Specific Process Knowledge/Etch/III-V ICP/SiO2: Difference between revisions

From LabAdviser
Bghe (talk | contribs)
No edit summary
Bghe (talk | contribs)
No edit summary
Line 40: Line 40:
|Selectivity to  resist [:1]
|Selectivity to  resist [:1]
|Not known
|Not known
|-
|Etch rate in silicon
|
bghe@Nanolab 20190117
*35 nm/min (middle of the wafers with 80% load)
*36 nm/min (edge of the wafers with 80% load)
|-
|-
|Wafer uniformity (100mm)
|Wafer uniformity (100mm)

Revision as of 16:07, 18 January 2019

Feedback to this page: click here

Parameter Parameter settings
Coil Power [W] 200
Platen Power [W] 25
Platen temperature [oC] 20
CF4 flow [sccm] 20
H2 flow [sccm] 10
Pressure [mTorr] 3


Results SiO2 Etch Slow Test by Artem Shikin @ Fotonik
Etch rate of PECVD BPSG 39.4nm/min (22-01-2016)
Etch rate in thermal oxide 48nm/min (bghe 17-01-2017)- whole 4" wafer with capton tape
Selectivity to resist [:1] Not known
Etch rate in silicon

bghe@Nanolab 20190117

  • 35 nm/min (middle of the wafers with 80% load)
  • 36 nm/min (edge of the wafers with 80% load)
Wafer uniformity (100mm) Not known
Profile [o] Not known
Wafer uniformity map (click on the image to view a larger image) Not known
SEM profile images NONE
Comment Tested on a plane BPSG layer. The etch rate is much lower for an etch time of e.g. 5s