!Parameter | !Parameter | ||
!Recipe on ICP metal: A SiO2 etch with C4F8 with resist mask | !Recipe on ICP metal: A SiO2 etch with C4F8 with resist mask | ||
|- | |- | ||
|Coil Power [W] | |Coil Power [W] | ||
|1000 | |1000 | ||
|- | |- | ||
|Platen Power [W] | |Platen Power [W] | ||
|200 | |200 | ||
|- | |- | ||
|Platen temperature [<sup>o</sup>C] | |Platen temperature [<sup>o</sup>C] | ||
|0 | |0 | ||
|- | |- | ||
|C<sub>4</sub>F<sub>8</sub> flow [sccm] | |C<sub>4</sub>F<sub>8</sub> flow [sccm] | ||
|10 | |10 | ||
|- | |- | ||
|H<sub>2</sub> flow [sccm] | |H<sub>2</sub> flow [sccm] | ||
|28 | |28 | ||
|- | |- | ||
|Pressure [mTorr] | |Pressure [mTorr] | ||
|2.5 | |2.5 | ||
|- | |- | ||
| Line 125: | Line 118: | ||
|-style="background:Black; color:White" | |-style="background:Black; color:White" | ||
!Results | !Results | ||
!Test | !Test | ||
|- | |- | ||
|Etch rate of thermal oxide | |Etch rate of thermal oxide | ||
|'''145-172 nm/min''' ''by bghe@danchip (2015-06-02)'' | | | ||
*'''145-172 nm/min''' ''by bghe@danchip (2015-06-02)'' | |||
*'''145 nm/min ''' ''by Martin Lind Ommen (fall 2016)'' | |||
|- | |- | ||
|Selectivity to resist [:1] | |Selectivity to resist [:1] | ||
| 4-5:1 (SiO2:resist) | | 4-5:1 (SiO2:resist) ''by bghe@danchip (2015-06-02)'' | ||
|- | |- | ||
|Cr etch rate | |Cr etch rate | ||
|1.6 nm/min (1:90 to SiO2) ''by Martin Lind Ommen (fall 2016)'' | |1.6 nm/min (1:90 to SiO2) ''by Martin Lind Ommen (fall 2016)'' | ||
|- | |- | ||
|Profile [<sup>o</sup>] | |Profile [<sup>o</sup>] | ||
|86-87 dg | |86-87 dg ''by bghe@danchip (2015-06-02)'' | ||
|- | |- | ||
|Wafer uniformity map (click on the image to view a larger image) | |Wafer uniformity map (click on the image to view a larger image) | ||
| | | | ||
|- | |- | ||
|SEM profile images | |SEM profile images | ||
|[[File:ICP metal s007592_21.jpg|200px]] [[File:ICP metal s007592_24.jpg|200px]] | |[[File:ICP metal s007592_21.jpg|200px]] [[File:ICP metal s007592_24.jpg|200px]]<br> ''by bghe@danchip (2015-06-02)'' | ||
| | | | ||
|- | |- | ||
|Etch rate in barc | |Etch rate in barc | ||
| | | | ||
|- | |- | ||
|Etch rate in KRF resist | |Etch rate in KRF resist | ||
|34 nm/min | |34 nm/min ''by bghe@danchip (2015-06-02)'' | ||
|- | |- | ||
|Comments | |Comments | ||
|Sample: s007592 | | | ||
*Sample: s007592 ''by bghe@danchip (2015-06-02)'' | |||
*See Martin Lind Ommen's results with hard masks in Process2share: [http://process2share.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Etching_of_SiO2] <br> There were problems with polymer on the surface after etching. | |||
|} | |} | ||
Revision as of 11:44, 20 January 2017
Feedback to this page: click here
It is possible to etch SiO2 in the ICP metal etcher but it is not designed for it and the results are not fantastic. It is a challenge to get a good selectivity to resist (typically in the range of 1:1 or worse) and it is probably not possible to get a profile angle of 90 degrees. More likely about 75-85 degrees. Different chemistries can be applied either based on CF4 or C4F8. If seems that C4F8 can give the best selectivity to resist (best case I have seem was 1:11 but it depends a lot on the process parameters)). If low coil power is needed CF4 chemistry is used because C4F8 needs a higher power to generate a plasma. /bghe 2016-04-25
Slow etch of SiO2 with resist as masking material - using a 6" carrier wafer with recess
This recipe can be used for slow etching of SiO2 with resist as masking material. Here are some test results presented.
| Parameter | Resist mask |
|---|---|
| Coil Power [W] | 200 |
| Platen Power [W] | 25 |
| Platen temperature [oC] | 0 |
| CF4 flow [sccm] | 20 |
| H2 flow [sccm] | 10 |
| Pressure [mTorr] | 3 |
SiO2 etch using DUV mask
Two chemistry regimes has been explored: One using CF4 and one using C4F8
- CF4: bad selectivity to the resist mask.
- C4F8: Better selectivity to the resist mask can be achieved
- Tests done by Peixiong
- Tests done by Berit
- Test by Zhibo Li @Danchip dec. 2016 - based on the work of Peixiong and Berit: File:Zhibo Li SiO2 ICP etch (dose205).docx
| Parameter | Recipe on ICP metal: A SiO2 etch with C4F8 with resist mask |
|---|---|
| Coil Power [W] | 1000 |
| Platen Power [W] | 200 |
| Platen temperature [oC] | 0 |
| C4F8 flow [sccm] | 10 |
| H2 flow [sccm] | 28 |
| Pressure [mTorr] | 2.5 |
| Results | Test | |
|---|---|---|
| Etch rate of thermal oxide |
| |
| Selectivity to resist [:1] | 4-5:1 (SiO2:resist) by bghe@danchip (2015-06-02) | |
| Cr etch rate | 1.6 nm/min (1:90 to SiO2) by Martin Lind Ommen (fall 2016) | |
| Profile [o] | 86-87 dg by bghe@danchip (2015-06-02) | |
| Wafer uniformity map (click on the image to view a larger image) | ||
| SEM profile images | by bghe@danchip (2015-06-02) |
|
| Etch rate in barc | ||
| Etch rate in KRF resist | 34 nm/min by bghe@danchip (2015-06-02) | |
| Comments |
|
SiO2 etch nLOF
| Parameter | Resist mask |
|---|---|
| Coil Power [W] | 800 |
| Platen Power [W] | 100 |
| Platen temperature [oC] | 0 |
| CF4 flow [sccm] | 30 |
| H2 flow [sccm] | 10 |
| Pressure [mTorr] | 4 |
| Results | Test on wafer with 50% load (Travka 50), by BGHE @danchip |
|---|---|
| Etch rate of thermal oxide | >110 nm/min (50% etch load) (09-03-2015) |
| Selectivity to resist [:1] | <0.7:1 (SiO2:resist) |
| Wafer uniformity (100mm) | Not known |
| Profile [o] | Not known |
| Wafer uniformity map (click on the image to view a larger image) | Not known |
| SEM profile images | NONE |
| Etch rate in nLOF resist | 1.6µm was removed after 10min |
| Comment | After 10min etch the resist was gone and the etch depth as 1.145µm in the oxide |
SiO2 etch with e-beam resist
| Process flow |
|---|
px1283lablejan1542014t1 250uc at 40mm x y pxline400p1000jan142014dt2 y= -40 -45 -50 -55mm dose 200 240 280 320uc
|
| Parameter | Resist mask |
|---|---|
| Coil Power [W] | 800 |
| Platen Power [W] | 150 |
| Platen temperature [oC] | -10 |
| C4F8 flow [sccm] | 8 |
| H2 flow [sccm] | 30 |
| Pressure [mTorr] | 2.5 |
| Results | Test on 6" wafer, by Peixiong Shi@danchip |
|---|---|
| Etch rate of thermal oxide | 131 nm/min (15-01-2014) |
| Selectivity to resist [:1] | ~1.8:1 (SiO2:resist) |
| Profile [o] | Not measured |
| Wafer uniformity map (click on the image to view a larger image) | Not known |
| SEM images |
|