Jump to content

Specific Process Knowledge/Thin film deposition/Deposition of Aluminium: Difference between revisions

From LabAdviser
Paphol (talk | contribs)
Paphol (talk | contribs)
Line 35: Line 35:
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Alcatel|Alcatel]])
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Alcatel|Alcatel]])
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]])
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]])
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Multisource PVD|PVD co-sputter/evaporation]])
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Multisource PVD|PVD co-sputter/evaporation]])
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]])
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]])
! Thermal evaporation ([[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]])
! Thermal evaporation ([[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]])
Line 43: Line 41:
! General description
! General description


|
E-beam deposition of Aluminium
|
|
E-beam deposition of Aluminium
E-beam deposition of Aluminium
|
|
E-beam deposition of Aluminium
E-beam deposition of Aluminium
|
Sputter deposition of Aluminium
|
|
Sputter deposition of Aluminium
Sputter deposition of Aluminium
Line 60: Line 54:
! Pre-clean
! Pre-clean
|RF Ar clean
|RF Ar clean
|RF Ar clean
|RF Ar clean
|RF Ar clean  
|RF Ar clean  
|RF Ar clean
|RF Ar clean
Line 70: Line 62:
|10Å to 1µm*
|10Å to 1µm*
|10Å to 1 µm*
|10Å to 1 µm*
|10Å to 1000 Å
|10Å to about 2000 Å
|10Å to ~0.5µm (very time consuming )
|10Å to ~0.5µm (very time consuming )
|10Å to 0.5 µm (this uses all Al in the boat)
|10Å to 0.5 µm (this uses all Al in the boat)
|-
|-
|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
! Deposition rate
! Deposition rate
|2Å/s to 15Å/s
|2Å/s to 15Å/s
|10Å/s to 15Å/s
|10Å/s to 15Å/s
|About 1Å/s
|Dependent on [[/Sputter rates for Al PVD co-sputter/evaporation|process parameters]] (about 1 Å/s).
|Depending on [[/Sputter rates for Al|process parameters]], up to ~2.5 Å/s
|Depending on [[/Sputter rates for Al|process parameters]], up to ~2.5 Å/s
|~2Å/s to 15Å/s
|~2Å/s to 15Å/s
|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
! Batch size
! Batch size
Line 97: Line 81:
*6x4" wafers or
*6x4" wafers or
*6x6" wafers
*6x6" wafers
|
*12x2" wafers or
*12x4" wafers or
*4x6" wafers
|
*12x4" wafers or
*12x4" wafers or
*4x6" wafers
|
|
*24x2" wafers or  
*24x2" wafers or  
Line 127: Line 103:
* Pyrex wafers  
* Pyrex wafers  


|
* Silicon wafers
* Quartz wafers
* Pyrex wafers
|
* Silicon wafers
* Quartz wafers
* Pyrex wafers


|  
|  
Line 168: Line 135:
* Metals  
* Metals  


|
* Silicon oxide
* Silicon (oxy)nitride
* Photoresist
* PMMA
* Mylar
* SU-8
* Metals
|
* Silicon oxide
* Silicon (oxy)nitride
* Photoresist
* PMMA
* Mylar
* SU-8
* Metals


|
|
Line 210: Line 159:
|Thickness above 200 nm: ask for permission
|Thickness above 200 nm: ask for permission
|Thickness above 200 nm: ask for permission
|Thickness above 200 nm: ask for permission
|Only very thin layers (up to 100 nm).
|Al sputter target: 99.995% Al
| 
| 
| 
| 

Revision as of 11:05, 19 September 2016


Feedback to this page: click here


Deposition of Aluminium

Aluminium can be deposited by e-beam evaporation, by sputtering and by thermal evaporation. In the chart below you can compare the different methods on the different deposition equipment.


Sputtering of Aluminium

Aluminium may be sputter deposited in either Wordentec of PVD co-sputter/evaporation

Thermal deposition of Aluminium

In Wordentec Aluminium can be deposited by Thermal deposition



E-beam evaporation (Alcatel) E-beam evaporation (Wordentec) Sputter deposition (Wordentec) Thermal evaporation (Wordentec)
General description

E-beam deposition of Aluminium

E-beam deposition of Aluminium

Sputter deposition of Aluminium

Aluminum deposition onto unexposed e-beam resist

Pre-clean RF Ar clean RF Ar clean RF Ar clean RF Ar clean
Layer thickness 10Å to 1µm* 10Å to 1 µm* 10Å to ~0.5µm (very time consuming ) 10Å to 0.5 µm (this uses all Al in the boat)
Deposition rate 2Å/s to 15Å/s 10Å/s to 15Å/s Depending on process parameters, up to ~2.5 Å/s ~2Å/s to 15Å/s
Batch size
  • Up to 1x4" wafers
  • smaller pieces
  • 24x2" wafers or
  • 6x4" wafers or
  • 6x6" wafers
  • 24x2" wafers or
  • 6x4" wafers or
  • 6x6" wafers
  • 24x2" wafers or
  • 6x4" wafers or
  • 6x6" wafers
Allowed substrates
  • Silicon wafers
  • Quartz wafers
  • Pyrex wafers
  • Silicon wafers
  • Quartz wafers
  • Pyrex wafers


  • Silicon wafers
  • Quartz wafers
  • Pyrex wafers
  • Silicon wafers
  • Quartz wafers
  • Pyrex wafers
Allowed materials
  • Silicon oxide
  • Silicon (oxy)nitride
  • Photoresist
  • PMMA
  • Mylar
  • SU-8
  • Metals


  • Silicon oxide
  • Silicon (oxy)nitride
  • Photoresist
  • PMMA
  • Mylar
  • SU-8
  • Metals


  • Silicon oxide
  • Silicon (oxy)nitride
  • Photoresist
  • PMMA
  • Mylar
  • SU-8
  • Metals


  • Silicon oxide
  • Silicon (oxy)nitride
  • Photoresist
  • PMMA
  • Mylar
  • SU-8
  • Metals
Comment Thickness above 200 nm: ask for permission Thickness above 200 nm: ask for permission    

* For thicknesses above 200 nm permission from ThinFilm group (thinfilm@danchip.dtu.dk) is required.

Aluminium deposition on ZEP520A for lift-off

This is a small study of which aluminium deposition that is best for aluminium lift-off on ZEP520A resist and a very thin layer of aluminium (~20nm).

The conclusion was that e-beam evaporation of aluminium in the Alcatel at 15Å/s gave the best result.

See details of the study here.


Aluminium deposition on AZ5214 for lift-off

Negative photolithographi process is recomended.

Positive photolithographi process from 1,5µ is possible especially for thin layers of metal.

The more pattern the easyer lift.


It was tried(jan09) to lift 2,5µ Al on 4,2µ negative resist on top of 11µ Apox SiO2 in acetone sonic-bath. This process was done in steps evaporating 5000Å a time with 5min pause and pressure down to at least 2E-6.


Comparison of roughness and other surface characteristics for different methods of Aluminium deposition

Studies by AFM was performed to examine differences in characteristics of the Al films, deposited with the differnt methods (sputter, e-beam, thermal). See details of the study here.