Specific Process Knowledge/Thin film deposition/ALD Picosun R200/ALD multilayers: Difference between revisions
| Line 95: | Line 95: | ||
image:Al2O3_LT_RI.JPG| Measured refractive index distribution across 100 mm wafer. | image:Al2O3_LT_RI.JPG| Measured refractive index distribution across 100 mm wafer. | ||
</gallery> | </gallery> | ||
<br clear="all" /> | |||
<b>Evgeniy Shkondin, DTU Danchip, 2014-2016.</b> | |||
<br clear="all" /> | |||
<br clear="all" /> | |||
==Low temperature deposition of TiO<sub>2</sub>== | ==Low temperature deposition of TiO<sub>2</sub>== | ||
Revision as of 18:06, 19 May 2016
This page describes non standart recipes including multilayers structures.
Low temperature deposition of Al2O3
Recipe: Al2O3 LT
Temperature: 80-150 oC
| TMA | H2O | |
|---|---|---|
| Nitrogen flow | 150 sccm | 200 sccm |
| Pulse time | 0.1 s | 0.2 s |
| Purge time | 5.0 s | 10.0 s |
Deposition rate: 0.089 nm/cycle (@120 oC)
This recipe has been developd for fabrication of high quality homogenious optical layers at low temperature.
| Al2O3 deposition at 120 oC | |||||||||||||||||||||||||||||||
|
| |||||||||||||||||||||||||||||||
%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%
The uniformity, thickness, refractive index has been obtained using Ellipsometer VASE.
-
Measured thickness distribution across 100 mm wafer.
-
Measured refractive index distribution across 100 mm wafer.
Evgeniy Shkondin, DTU Danchip, 2014-2016.
Low temperature deposition of TiO2
Recipe: TiO2 LT
Temperature: 80-150 oC
| TiCl4 | H2O | |
|---|---|---|
| Nitrogen flow | 150 sccm | 200 sccm |
| Pulse time | 0.2 s | 0.2 s |
| Purge time | 10.0 s | 15.0 s |
Deposition rate: 0.048 nm/cycle (@ 120 oC)
This recipe has been developd for fabrication of high quality homogenious optical layers at low temperature. The deposited TiO2 layers are amorphous.
| TiO2 deposition at 120 oC | |||||||||||||||||||||||||||||||
|
| |||||||||||||||||||||||||||||||
%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%
Low temperature grown multilayers on flat surfaces
Recipe: EMA01
Recipe: EMA02
Recipe: EMA03
Recipe: EMA04
Temperature: 120 oC
Al2O3/TiO2 multilayers on high aspect ratio structures
Recipe: Multi T
Temperature: 150 oC
-
Al2O3/TiO2 multilayers grown on silicon trenches.
Evgeniy Shkondin, DTU Danchip, 2014-2016.