Specific Process Knowledge/Lithography/DUVStepperLithography: Difference between revisions
Appearance
| Line 109: | Line 109: | ||
'''Standard processes:''' | '''Standard processes:''' | ||
BARC DUV42s-6 | |||
*'''(1001) DCH 150mm BARC 65nm''' Dispense 3ml@1000rpm; spin-off 60s@4700rpm; softbake 60s@175°C | *'''(1001) DCH 150mm BARC 65nm''' Dispense 3ml@1000rpm; spin-off 60s@4700rpm; softbake 60s@175°C | ||
*'''(1002) DCH 100mm BARC 65nm''' Dispense 1.6ml@1000rpm; spin-off 60s@4700rpm; softbake 60s@175°C | *'''(1002) DCH 100mm BARC 65nm''' Dispense 1.6ml@1000rpm; spin-off 60s@4700rpm; softbake 60s@175°C | ||
KRF M230Y | |||
*'''(1011) DCH 150mm M230Y 360nm''' Dispense 3.9ml@1000rpm; spin-off 60s@2500rpm; softbake 90s@130°C | *'''(1011) DCH 150mm M230Y 360nm''' Dispense 3.9ml@1000rpm; spin-off 60s@2500rpm; softbake 90s@130°C | ||
*'''(1012) DCH 100mm M230Y 360nm''' Dispense 1ml@1000rpm; spin-off 60s@2500rpm; softbake 90s@130°C | *'''(1012) DCH 100mm M230Y 360nm''' Dispense 1ml@1000rpm; spin-off 60s@2500rpm; softbake 90s@130°C | ||
KRF M35G | |||
*'''(1021) DCH 150mm M35G 750nm''' | *'''(1021) DCH 150mm M35G 750nm''' | ||
*'''(1022) DCH 100mm M35G 750nm''' | *'''(1022) DCH 100mm M35G 750nm''' | ||