Jump to content

Specific Process Knowledge/Thin film deposition/Furnace LPCVD Nitride: Difference between revisions

From LabAdviser
Pevo (talk | contribs)
Pevo (talk | contribs)
Line 37: Line 37:


==Equipment performance and process related parameters==
==Equipment performance and process related parameters==
[[image:Under_construction.png|50px]]


==<span style="color:Red">From April 2016 the processed on the LPCVD nitride furnaces have been changed, so that only stoichiometric nitride is deposited in the 4" nitride furnace, and only low stress (silicon rich) nitride is deposited in the 6" nitride furnace</span>==
==<span style="color:Red">From April 2016 the processed on the LPCVD nitride furnaces have been changed, so that only stoichiometric nitride is deposited in the 4" nitride furnace, and only low stress (silicon rich) nitride is deposited in the 6" nitride furnace</span>==

Revision as of 11:33, 4 May 2016

Feedback to this page: click here

6" LPCVD nitride furnace (E3) located in cleanroom E-6
4" LPCVD nitride furnace (B2) located in cleanroom B-1

Deposition of Silicon Nitride using LPCVD

Danchip has two LPCVD (Low Pressure Chemical Vapour Deposition) furnaces that are dedicated for deposition of silicon nitride: A 6" furnace (installed in 2008) for deposition of stoichiometric nitride on 100 mm and 150 mm wafers and a 4" furnace (installed in 1995) that is mainly used for deposition of silicon rich (i.e. low stress) nitride on 100 mm wafers. In LabManager the two furnaces are named "Furnace: LPCVD nitride (6") (E3)" and "Furnace: LPCVD nitride (4") (B2)", respectively. Both furnaces are Tempress horizontal furnaces.

Please be aware of that it is not allowed to deposit silicon rich nitride in the 6" nitride furnace to avoid problems with particles. The 4" nitride furnace is mainly dedicated for deposition of silicon rich nitride which does affect the cleanliness of the furnace. And please check the cross contamination information in LabManager before you use any of the two furnaces.

The LPCVD silicon nitride deposition is a batch process, where nitride can be deposited on a batch of up to 25 wafers (in the 6" nitride furnace) or 15 wafers (in the 4" nitride furnace) at a time. The deposition takes place under vacuum (120-200 mTorr, depending on the process) and at temperature (780-845 C, depending on the process). The reactive gases are ammonia (NH3) and dichlorsilane (SiH2Cl2). The LPCVD nitride has a very good step coverage, and the film thickness is very uniform over the wafers.

The user manuals, quality control procedures and results, user APVs, technical information and contact information can be found in LabManager:

4" LPCVD nitride furnace (B2),

6" LPCVD nitride furnace (E3)


Process information

Equipment performance and process related parameters

From April 2016 the processed on the LPCVD nitride furnaces have been changed, so that only stoichiometric nitride is deposited in the 4" nitride furnace, and only low stress (silicon rich) nitride is deposited in the 6" nitride furnace

Equipment 4" LPCVD nitride furnace (B2) 6" LPCVD nitride furnace (E3)
Purpose Deposition of
  • Silicon rich (low stress) nitride
  • (Stoichiometric nitride)
  • Stoichiometric nitride
Performance Step coverage
  • Very good
  • Very good
Film quality
  • Deposition on both sides of the substrate
  • Dense film
  • Few defects
  • Deposition on both sides of the substrate
  • Dense film
  • Very few defects
Process parameter range Temperature
  • 830-845 oC

The temperature vary over the furnace tube

  • 780-790 oC

The temperature very over the furnace tube

Pressure
  • 120 mTorr
  • 200 mTorr
Gas flows
  • Dichlorsilane (SiH2Cl2): 80 sccm
  • Ammonia (NH3): 20 sccm
  • Dichlorsilane (SiH2Cl2): 10-45 sccm
  • Ammonia (NH3): 160-180 sccm

The gas flows depend on whether nitride is deposited on 4" or 6" wafers

Substrates Batch size
  • 1-15 100 mm wafers

Including a test wafer

  • 1-25 100 mm wafers
  • 1-25 150 mm wafers

Including a test wafer

Allowed materials
  • Silicon wafers (new or RCA cleaned)
    • with layers of silicon oxide or silicon (oxy)nitride
    • from the A, B and E stack furnaces
  • Quartz/fused silica wafers (RCA cleaned)
  • Silicon wafers (new or RCA cleaned)
    • with layers of silicon oxide or silicon (oxy)nitride
    • from the A, B and E stack furnaces
  • Quartz/fused silica wafers (RCA cleaned)