Jump to content

Specific Process Knowledge/Etch/Etching of Chromium: Difference between revisions

From LabAdviser
BGE (talk | contribs)
Mbe (talk | contribs)
Line 63: Line 63:
|
|
No restrictions.
No restrictions.
Make a note on the beaker of which materials have been processed.
Make a note on the bottle of which materials have been processed.
|-
|-
|}
|}

Revision as of 15:45, 7 November 2008

Etching of Chromium

Fume hood: positioned in cleanroom 2.
Wet Etch of Chromium can take place in a beaker in this fume hood

Etching of chromium is done wet at Danchip making your own set up in a beaker in a fume hood - preferably in cleanroom 2 or 4. We have two solution for this:

  1. HNO3:H2O:cerisulphate - 90ml:1200ml:15g - standard at Danchip
  2. Commercial chromium etch

Etch rate are depending on the level of oxidation of the metal.


Overview of the data for the chromium etches

Chromium etch 1 Chromium etch 2
General description

Etch of chromium

Etch of chromium

Chemical solution HNO3:H2O:cerisulphate - 90ml:1200ml:15g Commercial chromium etch

CE 8002-A

Process temperature Room temperature Room temperature
Possible masking materials

Photoresist (1.5 µm AZ5214E)

Photoresist (1.5 µm AZ5214E)

Etch rate

~40-100 nm/min

~10-20 nm/min

Batch size

1-25 wafers at a time

1-25 wafer at a time

Size of substrate

4" wafers

4" wafers

Allowed materials

No restrictions. Make a note on the beaker of which materials have been processed.

No restrictions. Make a note on the bottle of which materials have been processed.