It consists of two solutions: RCA1 and RCA2 plus diluted HF. A crucial part of the RCA clean is the oxidation by H<math>_2</math>O<math>_2</math>. Therefore the life time of the RCA solutions are limited by the presence of the H<math>_2</math>O<math>_2</math> which is highly volatile at 70 <math>^o</math>C.
It consists of two solutions: RCA1 and RCA2 plus diluted HF. A crucial part of the RCA clean is the oxidation by H<math>_2</math>O<math>_2</math>. Therefore the life time of the RCA solutions are limited by the presence of the H<math>_2</math>O<math>_2</math> which is highly volatile at 70 <math>^o</math>C.


The RCA1 contains: H<math>_2</math>O, NH<math>_4</math>OH and H<math>_2</math>O<math>_2</math> (5:1:1). It is used for removal of light organics, particles and metal. <br \>
*The RCA1 contains: H<math>_2</math>O, NH<math>_4</math>OH and H<math>_2</math>O<math>_2</math> (5:1:1). It is used for removal of light organics, particles and metal. <br \>
The RCA2 contains: H<math>_2</math>O, HCl and H<math>_2</math>O<math>_2</math> (5:1:1). It is used for removal of heavy metals, alkalies and metal hydroxides.
*The RCA2 contains: H<math>_2</math>O, HCl and H<math>_2</math>O<math>_2</math> (5:1:1). It is used for removal of heavy metals, alkalies and metal hydroxides.


===RCA procedure===
===RCA procedure===

Revision as of 11:02, 4 March 2008

RCA cleaning

The RCA clean is used for cleaning the wafers before taking them into the furnaces and a few other equipments (check the cross contamination sheet). It consists of two solutions: RCA1 and RCA2 plus diluted HF. A crucial part of the RCA clean is the oxidation by H2O2. Therefore the life time of the RCA solutions are limited by the presence of the H2O2 which is highly volatile at 70 oC.

  • The RCA1 contains: H2O, NH4OH and H2O2 (5:1:1). It is used for removal of light organics, particles and metal.
  • The RCA2 contains: H2O, HCl and H2O2 (5:1:1). It is used for removal of heavy metals, alkalies and metal hydroxides.

RCA procedure

  • RCA1: 10 min
  • DI water rinsing (dumping three times)
  • HF: 30 sec (avoid it if you have oxide as the top layer)
  • DI water rinsing (dumping three times)
  • RCA2: 10 min
  • DI water rinsing (dumping three times)
  • Optional: HF: 30 sec (avoid it if you have oxide as the top layer)
  • DI water rinsing (dumping three times)

For procedure details please look in the user manual positioned in LabManager.

Overview of RCA process data

RCA1 RCA2 HF
General description

It is used for removal of light organics, particles and metal.

It is used for removal of heavy metals, alkalies and metal hydroxides.

It is used for removal of oxide generated in RCA1 and RCA2

Chemical solution H2O, NH4OH(29%) and H2O2(30%) (5:1:1) H2O, HCl(37%) and H2O2(30%) (5:1:1) 5% HF
Process temperature 70-80 oC 70-80 oC Room temperature
Process time

10 min.

10 min.

30 sec.

Life time of the chemical solutions Can only be heated one time. When hot: it lasts for ~1h Can only be heated one time. When hot: it lasts for ~1h ~2 months
Allowed materials
  • Silicon
  • Silicon oxide
  • Silicon nitride
  • Quartz wafers/fused silica
  • Silicon
  • Silicon oxide
  • Silicon nitride
  • Quartz wafers/fused silica
  • Silicon
  • Silicon oxide
  • Silicon nitride
Batch size

1-25 2",4" or 6" wafers at a time

1-25 2",4" or 6" wafers at a time

1-25 2",4" or 6" wafers at a time

Size of substrate

2"-4"-6" wafers

2"-4"-6" wafers

2"-4"-6" wafers