Specific Process Knowledge/Wafer cleaning/RCA: Difference between revisions
| Line 14: | Line 14: | ||
*RCA2: 10 min | *RCA2: 10 min | ||
*DI wafer rinsing (dumping three times) | *DI wafer rinsing (dumping three times) | ||
*HF: 30 sec (avoid it if you have oxide as the top layer) | *Optional: HF: 30 sec (avoid it if you have oxide as the top layer) | ||
*DI wafer rinsing (dumping three times) | *DI wafer rinsing (dumping three times) | ||
===Overview of RCA process data=== | ===Overview of RCA process data=== | ||
Revision as of 09:48, 4 March 2008
RCA cleaning
The RCA clean is used for cleaning the wafers before taking them into the furnaces and a few other equipments (check the cross contamination sheet). It consists of two solutions: RCA1 and RCA2 plus diluted HF.
The RCA1 contains: HO, NHOH and HO (5:1:1). It is used for removed of light organics, particles and metal.
The RCA2 contains: HO, HCl and HO (5:1:1). It is used for removal of heavy metals, alkalies and metal hydroxides.
RCA procedure
- RCA1: 10 min
- DI wafer rinsing (dumping three times)
- HF: 30 sec (avoid it if you have oxide as the top layer)
- DI wafer rinsing (dumping three times)
- RCA2: 10 min
- DI wafer rinsing (dumping three times)
- Optional: HF: 30 sec (avoid it if you have oxide as the top layer)
- DI wafer rinsing (dumping three times)
Overview of RCA process data
| RCA1 | RCA2 | HF | |
|---|---|---|---|
| General description |
It is used for removal of light organics, particles and metal. |
It is used for removal of light organics, particles and metal. |
It is used for removal of oxide generated in RCA1 and RCA2 |
| Chemical solution | HO, NHOH(29%) and HO(30%) (5:1:1) | HO, HCl(37%) and HO(30%) (5:1:1) | 5% HF |
| Process temperature | 70-80 oC | 70-80 oC | Room temperature |
| Process time |
10 min. |
10 min. |
30 sec. |
| Life time of the chemical solutions | Can only be heated one time. When hot: it lasts for ~1h | Can only be heated one time. When hot: it lasts for ~1h | ~2 months |
| Allowed materials |
|
|
|
| Batch size |
1-25 2",4" or 6" wafers at a time |
1-25 2",4" or 6" wafers at a time |
1-25 2",4" or 6" wafers at a time |
| Size of substrate |
2"-4"-6" wafers |
2"-4"-6" wafers |
2"-4"-6" wafers |