Specific Process Knowledge/Thin film deposition/PECVD/Doping: Difference between revisions

From LabAdviser
Kabi (talk | contribs)
Kabi (talk | contribs)
No edit summary
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/PECVD/Doping  click here]'''  
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/PECVD/Doping  click here]'''  


=<span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>[[image:Under_construction.png|200px]]=


==Boron-doping by use of BSG glass deposited in PECVD2==
==Boron-doping by use of BSG glass deposited in PECVD2==

Revision as of 14:04, 1 December 2015

Feedback to this page: click here


Boron-doping by use of BSG glass deposited in PECVD2

Results from Joachim Dahl Thomsen, Nanotech, 2014

Recipe

Recipe name SiH4 flow [sccm] N2O flow [sccm] N2 flow [sccm] B2H6 flow [sccm] PH3 flow [sccm] Pressure [mTorr] Power [W] Description
1PBSG 17 1600 0 120, 130, 140, 160, 240 0 400 380 BSG glass for driving in boron in Silicon

5 tests were made where only the B2H6 flow was changed for each deposition (120sccm,130sccm,140sccm,160sccm,240sccm). All deposition times were 2 min, resulting in 440 nm Oxide. The wafers were annealed in Anneal Oxide Furnace (C1) at 1000°C for 85 min to drive in the boron and the oxide was subsequently etched in BHF. The wafers were then analyzed by SIMS and the results are shown in the figure below:


Boron concentration measured by SIMS. Results from Joachim Dahl Thomsen, Nanotech, 2014.


Boron-doping by use of BSG glass deposited in PECVD2

Results from Trine Holm Christensen, Space, Feb. 2015

Recipe

Recipe name SiH4 flow [sccm] N2O flow [sccm] N2 flow [sccm] B2H6 flow [sccm] PH3 flow [sccm] Pressure [mTorr] Power [W] Description
1PBSG 17 1600 0 120, 130, 140 0 400 380 BSG glass for driving in boron in Silicon

3 tests were made where only the B2H6 flow was changed for each deposition (120sccm,130sccm,140sccm,160sccm,240sccm). All deposition times were 2 min, resulting in 440 nm Oxide. The wafers were going through several annealing and oxidation step:

The total thermal budget for the wafers:

Anneal in Furnace (C1): ANN1000, 30 min in N2, strip of oxide in a 25 min BHF etch.

Wet oxidation in Furnace (C1): WET1050, 30 min, no further anneal

Anneal in Furnace (C1): ANN950, 60 min in N2

The wafers were then analyzed by SIMS and the results are shown in the figure below:

Boron concentration measured by SIMS. Results from Trine Holm Christensen, Space, Feb. 2015.

Measured peak concentrations and sheet resistances:

Wafer Peak Concentration

[atoms/cm3]

Sheet Resistance

[Ω/sq]

BSG120 1.75*1019 56.4
BSG130 2.44*1019 36.2
BSG140 2.36*1019 40.3