Jump to content

Specific Process Knowledge/Thin film deposition/Furnace LPCVD PolySilicon/Boron doped poly-Si and a-Si: Difference between revisions

From LabAdviser
Paphol (talk | contribs)
No edit summary
Paphol (talk | contribs)
No edit summary
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Furnace_LPCVD_PolySilicon/Boron_doped_poly-Si_and_a-Si click here]'''
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Furnace_LPCVD_PolySilicon/Boron_doped_poly-Si_and_a-Si click here]'''
[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Aluminium_Nitride/AlN_in_PVD_co-sputter click here]


==Boron-doped amorphous silicon by using 4" LPCVD polysilicon furnace (B4) ==
==Boron-doped amorphous silicon by using 4" LPCVD polysilicon furnace (B4) ==

Revision as of 15:18, 2 November 2015

Feedback to this page: click here

Boron-doped amorphous silicon by using 4" LPCVD polysilicon furnace (B4)

Result from Thomas Pedersen, @Nanotech, Sep 2015

Process parameters

Pressure: 250 mtorr

Temperature: 580 °C

Silane (SiH4) flow: Constant at 80 sccm

Diborane (B2H6) flow: Varied from 3 sccm to 40 sccm

Anneal: No annealing afterwards

Test wafer position: Center of the boat

Results

The Boron concentration of the film was controlled by the flow of B2H6 gas. To establish how boron doping concentration varied with B2H6 flow, films of silicon were deposited with B2H6 gas flows modulated during deposition to produce doping spikes. The two figures below show a typical SIMS concentration depth profile of a B2H6 modulation-doped film deposited on a Silicon dioxide substrate. During deposition, the gas flow of SiH4 was held constant, while flows of B2H6 was varied to create the dopant spikes.


Boron concentration measured by SIMS. Result from Thomas Pedersen, Nanotech, Sep 2015.