Specific Process Knowledge/Thermal Process/Furnace: Multipurpose annealing/Acceptance test: Difference between revisions
Appearance
No edit summary |
|||
| Line 7: | Line 7: | ||
Recipe: "vr_dryOx_1000C_120min_150_5Wafer_D1_mit_Inliner_oPurgering.ATV" | '''Recipe''': "vr_dryOx_1000C_120min_150_5Wafer_D1_mit_Inliner_oPurgering.ATV" | ||
Oxidation time: 80 min | '''Oxidation time''': 80 min | ||
Oxidation temperature: 1050 <sup>o</sup>C | |||
O<sub>2</sub> flow: 1 slm | '''Oxidation temperature''': 1050 <sup>o</sup>C (all temoperature zones) | ||
'''O<sub>2</sub> flow''': 1 slm | |||
The oxidation has been done with 150 mm wafer, and with 30 wafers in the furnace. | The oxidation has been done with 150 mm wafer, and with 30 wafers in the furnace. | ||
| Line 18: | Line 20: | ||
==Results== | ==Results== | ||
The oxide thickness has been measured in 13 points on each wafer using the M-2000V ellipsometer. | |||
{| border="2" cellpadding="2" cellspacing="1" style="text-align:center;" | {| border="2" cellpadding="2" cellspacing="1" style="text-align:center;" | ||
|- | |- | ||
! | ! | ||
! Date | ! Date | ||
! colspan="3" | Wafer 4 | ! colspan="3" | Wafer 4 | ||
! colspan="3" | Wafer 16 | ! colspan="3" | Wafer 16 | ||
! colspan="3" | Wafer 28 | ! colspan="3" | Wafer 28 | ||
! colspan="3" | Center point only | |||
|- | |- | ||
! width="80" | | ! width="80" | | ||
| Line 31: | Line 36: | ||
! width="50" | Average oxide thickness [nm] | ! width="50" | Average oxide thickness [nm] | ||
! width="50" | St. deviation | ! width="50" | St. deviation | ||
! width="50" | Non-uniformity [%] | |||
! width="50" | Average oxide thickness [nm] | |||
! width="50" | St. deviation | |||
! width="50" | Non-uniformity [%] | ! width="50" | Non-uniformity [%] | ||
! width="50" | Average oxide thickness [nm] | ! width="50" | Average oxide thickness [nm] | ||
| Line 50: | Line 58: | ||
| 0.8 | | 0.8 | ||
| 1.2 | | 1.2 | ||
| 107.0 | |||
| 2.1 | |||
| 1.9 | |||
|- | |- | ||
! Run 2 | ! Run 2 | ||
| Line 61: | Line 72: | ||
| 107.3 | | 107.3 | ||
| 0.7 | | 0.7 | ||
| 0.9 | |||
| 105.7 | |||
| 1.0 | |||
| 0.9 | | 0.9 | ||
|- | |- | ||
| Line 74: | Line 88: | ||
| 0.6 | | 0.6 | ||
| 1.1 | | 1.1 | ||
| 102.9 | |||
| 1.0 | |||
| 1.0 | |||
|- | |||
! Average | |||
| | |||
| 106.9 | |||
| 1.2 | |||
| 1.7 | |||
| 105.1 | |||
| 1.0 | |||
| 1.3 | |||
| 105.3 | |||
| 0.7 | |||
| 1.1 | |||
| 105.2 | |||
| 1.4 | |||
| 1.3 | |||
|- | |- | ||
! Common | ! Common | ||
| colspan="23" | Temperature 20 degs, HBC 10 torr, Short funnel, with baffle & 5mm spacers | | colspan="23" | Temperature 20 degs, HBC 10 torr, Short funnel, with baffle & 5mm spacers | ||
|} | |} | ||
Revision as of 09:14, 12 August 2015
THIS PAGE IS UNDER CONSTRUCTION
The acceptance for the Multipurpose Anneal furnace was performed in November 2014 by ATV Technologie.
Recipe: "vr_dryOx_1000C_120min_150_5Wafer_D1_mit_Inliner_oPurgering.ATV"
Oxidation time: 80 min
Oxidation temperature: 1050 oC (all temoperature zones)
O2 flow: 1 slm
The oxidation has been done with 150 mm wafer, and with 30 wafers in the furnace.
Wafer 4 (towards the door), wafer 16 and wafer 28 (towards the service area) were measured.
Results
The oxide thickness has been measured in 13 points on each wafer using the M-2000V ellipsometer.
| Date | Wafer 4 | Wafer 16 | Wafer 28 | Center point only | |||||||||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Average oxide thickness [nm] | St. deviation | Non-uniformity [%] | Average oxide thickness [nm] | St. deviation | Non-uniformity [%] | Average oxide thickness [nm] | St. deviation | Non-uniformity [%] | Average oxide thickness [nm] | St. deviation | Non-uniformity [%] | ||||||||||||
| Run 1 | 28-01-2015 | 109.7 | 1.0 | 1.7 | 107.7 | 0.9 | 1.1 | 106.5 | 0.8 | 1.2 | 107.0 | 2.1 | 1.9 | ||||||||||
| Run 2 | 28-01-2015 | 107.3 | 1.7 | 2.4 | 105.0 | 1.4 | 1.7 | 107.3 | 0.7 | 0.9 | 105.7 | 1.0 | 0.9 | ||||||||||
| Run 3 | 30-01-2015 | 103.6 | 0.8 | 1.1 | 102.6 | 0.6 | 1.2 | 102.2 | 0.6 | 1.1 | 102.9 | 1.0 | 1.0 | ||||||||||
| Average | 106.9 | 1.2 | 1.7 | 105.1 | 1.0 | 1.3 | 105.3 | 0.7 | 1.1 | 105.2 | 1.4 | 1.3 | |||||||||||
| Common | Temperature 20 degs, HBC 10 torr, Short funnel, with baffle & 5mm spacers | ||||||||||||||||||||||