Specific Process Knowledge/Thermal Process/Furnace: Multipurpose annealing/Acceptance test: Difference between revisions
Appearance
| Line 68: | Line 68: | ||
| 0.8 | | 0.8 | ||
| 1.1 | | 1.1 | ||
| | | 102.6 | ||
| | | 0.6 | ||
| | | 1.2 | ||
| | | 102.2 | ||
| | | 0.6 | ||
| | | 1.1 | ||
|- | |- | ||
! Common | ! Common | ||
| colspan="23" | Temperature 20 degs, HBC 10 torr, Short funnel, with baffle & 5mm spacers | | colspan="23" | Temperature 20 degs, HBC 10 torr, Short funnel, with baffle & 5mm spacers | ||
|} | |} | ||
Revision as of 08:56, 12 August 2015
THIS PAGE IS UNDER CONSTRUCTION
The acceptance for the Multipurpose Anneal furnace was performed in November 2014 by ATV Technologie.
Recipe: "vr_dryOx_1000C_120min_150_5Wafer_D1_mit_Inliner_oPurgering.ATV"
Oxidation time: 80 min Oxidation temperature: 1050 oC O2 flow: 1 slm
The oxidation has been done with 150 mm wafer, and with 30 wafers in the furnace.
Wafer 4 (towards the door), wafer 16 and wafer 28 (towards the service area) were measured.
Results
| Run number | Resist etch rate [nm/min] | Wafer 4 | Wafer 16 | Wafer 28 | |||||||||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Average oxide thickness [nm] | St. deviation | Non-uniformity [%] | Average oxide thickness [nm] | St. deviation | Non-uniformity [%] | Average oxide thickness [nm] | St. deviation | Non-uniformity [%] | |||||||||||||||
| Run 1 | 109.7 | 1.0 | 1.7 | 107.7 | 0.9 | 1.1 | 106.5 | 0.8 | 1.2 | ||||||||||||||
| Run 2 | 107.3 | 1.7 | 2.4 | 102.6 | 0.6 | 1.2 | 102.2 | 0.6 | 1.1 | ||||||||||||||
| Run 3 | 103.6 | 0.8 | 1.1 | 102.6 | 0.6 | 1.2 | 102.2 | 0.6 | 1.1 | ||||||||||||||
| Common | Temperature 20 degs, HBC 10 torr, Short funnel, with baffle & 5mm spacers | ||||||||||||||||||||||