Jump to content

Specific Process Knowledge/Etch/ICP Metal Etcher/Barc Etch: Difference between revisions

From LabAdviser
Bghe (talk | contribs)
Bghe (talk | contribs)
Line 26: Line 26:
! Results
! Results
|-  
|-  
|Etch rate in barc||52nm in 30s [bghe 20150519]
|Etch rate in barc||52nm in 30s ''[bghe 20150519]''
|-
|-
|Etch rate in KRF resist||27 nm in 30s [bghe 20150519]
|Etch rate in KRF resist||27 nm in 30s ''[bghe 20150519]''
|-  
|-  
|Selectivity KRF:Barc||1:2  
|Selectivity KRF:Barc||1:2  

Revision as of 13:35, 19 May 2015

Feedback to this page: click here

Barc Etch

Etching barc with a dedicated recipe for barc etching is a good idea if you are on the limit of having enough DUV resist mask to reach etch depth you need.Here is an example of a barc etch I have started testing.

Parameter Barc etch with CF4
Coil power 800W
Platen power 100W
Pressure 3 mTorr
Flow rate CF4 4 sccm
Flow rate H2 20sccm


Parameter Results
Etch rate in barc 52nm in 30s [bghe 20150519]
Etch rate in KRF resist 27 nm in 30s [bghe 20150519]
Selectivity KRF:Barc 1:2
Etch 65nm barc Use 40-45s