'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/ | '''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/ICP_Metal_Etcher/Barc_Etch click here]''' | ||
==Barc Etch== | ==Barc Etch== |
Revision as of 12:24, 19 May 2015
Feedback to this page: click here
Barc Etch
Etching barc with a dedicated recipe for barc etching is a good idea if you are on the limit of having enough DUV resist mask to reach etch depth you need.Here is an example of a barc etch I have started testing.
Parameter | Barc etch with CF4 |
---|---|
Coil power | 800W |
Platen power | 100W |
Pressure | 3 mTorr |
Flow rate CF4 | 4 sccm |
Flow rate H2 | 20sccm |
Parameter | Results |
---|---|
Etch rate in barc | 52nm in 30s |
Etch rate in KRF resist | 27 nm in 30s |
Selectivity KRF:Barc | 1:2 |
Etch 65nm barc | Use 40-45s |