== Field stitching == | == Field stitching == | ||
In this experiment, several writing fields (1 mm x 1 mm) were stitched together. Vernier | In this experiment, several writing fields (1 mm x 1 mm) were stitched together. Vernier scales on the edges of each writing field shows the field stitching bewteen fields. | ||
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 95%" | |||
|- | |||
|- | |||
|-style="background:Black; color:White" | |||
!colspan="6"|wafer 11.17 Stitching accuracy, Processed by TIGRE, April 2015 | |||
|- | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
!Resist | |||
!E-beam exposure | |||
!Development | |||
!Metallisation | |||
!Lift-off | |||
!Characterisation | |||
|- | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
|CSAR AR-P6200 AllResist, 400 rpm, 60s, softbaked 60s @ 150degC | |||
|JBX9500 E-2, 2nA aperture 5, dose 300 µC/cm2, L1: 1st set of Vernier scales on edges (North, Upper Right, East, Lower Right, South, Lower Left, West, Upper Left) of entire writi9ng field | |||
|AR-600-546, 60 s | |||
|5 nm Ti, 45 nm Au, Wordentec (D-2) | |||
|AR-600-71, 5-10 min, 4s ultrasonic (D-3) | |||
|Zeiss Supra 60VP, 10kV, Inlens detector | |||
|- | |||
|} | |||
[[File:FieldToField.png|700px]] | [[File:FieldToField.png|700px]] | ||