''Sequence names and process parameters (Sequence no. 1000-1999):''
''Sequence names and process parameters (Sequence no. 1000-1999):''
Single puddle:
*'''DCH 100mm SP 30s'''
*'''DCH 100mm SP 30s'''
*'''DCH 100mm SP 60s'''
*'''DCH 100mm SP 60s'''
*'''DCH 100mm SP 90s'''
*'''DCH 100mm SP 120s'''
*'''DCH 100mm SP 120s'''
*'''DCH 150mm SP 60s'''
*'''DCH 150mm SP 60s'''
Each of these sequences start with a 2s pre-wet at 1200 rpm using developer. The puddle dispense is done at a rotation of 30rpm. The dispense time is 3s, and 7s, corresponding to a volume of 11 ml, and 26 ml, for 100mm, and 150mm, respectively. The development (puddle time) is split in two by an agitation step of 2s at 30rpm (one rotation). Spin-off is 3s at 4000rpm. Finally, the wafer is rinsed as described above.
 
Multiple puddle:
*'''DCH 100mm MP 3x60s'''
*'''DCH 100mm MP 3x60s'''
*'''DCH 100mm MP 3x60s'''
 
Each of these sequences start with a 2s pre-wet at 1200 rpm using developer. The puddle dispense is done at a rotation of 30rpm. The dispense time is 3s, and 7s, corresponding to a volume of 11 ml, and 26 ml, for 100mm, and 150mm, respectively. The development (puddle time) is split in two by an agitation step of 2s at 30rpm (one rotation). Spin-off is 3s at 4000rpm. Finally, the wafer is rinsed as described above. The multiple puddle sequences repeat the dispense, development, and spin off steps a number of times before the rinse.
 
*'''DCH 100mm SP 60s no spinoff'''
*'''DCH 100mm SP 60s no spinoff'''
As DCH 100mm SP 60s except the spin-off step is omitted. The development is thus terminated by the rinse (30s @ 4000rpm). This may help in case of scumming problems.
As DCH 100mm SP 60s except the spin-off step is omitted. The development is thus terminated by the rinse (30s @ 4000rpm). This may help in case of scumming problems.