Specific Process Knowledge/Etch/Etching of Chromium: Difference between revisions
Appearance
| Line 1: | Line 1: | ||
==Etching of Chromium== | ==Etching of Chromium== | ||
[[Image: | [[Image:fumehoodetch-chrom.jpg|300x300px|thumb|Wet Aluminium Etch: Positioned in cleanroom 4]] | ||
Etching of chromium is done wet at Danchip making your own set up in a beaker in a fume hood - preferably in cleanroom 2 or 4. We have two solution for this: | Etching of chromium is done wet at Danchip making your own set up in a beaker in a fume hood - preferably in cleanroom 2 or 4. We have two solution for this: | ||
Revision as of 14:17, 5 February 2008
Etching of Chromium

Etching of chromium is done wet at Danchip making your own set up in a beaker in a fume hood - preferably in cleanroom 2 or 4. We have two solution for this:
- HNO:HO:cerisulphate - 90ml:1200ml:15g - standard at Danchip
- Commercial chromium etch
Etch rate are depending on the level of oxidation of the metal.
| Chromium etch 1 | Chromium etch 2 | |
|---|---|---|
| General description |
Etch of chromium |
Etch of chromium |
| Chemical solution | HNO:HO:cerisulphate - 90ml:1200ml:15g | Commercial chromium etch
CE 8002-A |
| Process temperature | Room temperature | Room temperature |
| Possible masking materials |
Photoresist (1.5 µm AZ5214E) |
Photoresist (1.5 µm AZ5214E) |
| Etch rate |
~40-100 nm/min |
~10-20 nm/min |
| Batch size |
1-25 wafers at a time |
1-25 wafer at a time |
| Size of substrate |
4" wafers |
4" wafers |
| Allowed materials |
No restrictions. Make a note on the beaker of which materials have been processed. |
No restrictions. Make a note on the beaker of which materials have been processed. |