Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange/ProcessA: Difference between revisions
No edit summary |
No edit summary |
||
Line 35: | Line 35: | ||
[[file:S004257-13.jpg|150px|frameless ]] | [[file:S004257-13.jpg|150px|frameless ]] | ||
[[file:S004257-14.jpg|150px|frameless ]] | [[file:S004257-14.jpg|150px|frameless ]] | ||
|- | |||
| 20/11-2014 | |||
| 4" Danchip QC Wafer | |||
| 1.5 µm AZ resist, daq2 mask | |||
| Si / 10 % | |||
| Pegasus/jmli | |||
| 10 minute TDESC clean, 10 minute PR strip post process | |||
| danchip/QC/QCprocA, 55 cycles (11+44) or 10:05 minutes | |||
| S004580 | |||
! OLD showerhead | |||
| | |||
[[file:S004580-01.jpg|150px|frameless ]] | |||
[[file:S004580-02.jpg|150px|frameless ]] | |||
[[file:S004580-03.jpg|150px|frameless ]] | |||
|- | |- | ||
| 1/12-2014 | | 1/12-2014 |
Revision as of 15:49, 17 December 2014
Date | Substrate Information | Process Information | SEM Images | ||||||
---|---|---|---|---|---|---|---|---|---|
Wafer info | Mask | Material/ Exposed area | Tool / Operator | Conditioning | Recipe | Wafer ID | Comments | ||
18/8-2014 | 4" Danchip QC Wafer | 1.5 µm AZ resist, daq2 mask | Si / 10 % | Pegasus/jmli | 10 minute TDESC clean, 10 minute PR strip post process | danchip/QC/QCprocA, 55 cycles (11+44) or 10:05 minutes | S004257 | OLD showerhead | |
20/11-2014 | 4" Danchip QC Wafer | 1.5 µm AZ resist, daq2 mask | Si / 10 % | Pegasus/jmli | 10 minute TDESC clean, 10 minute PR strip post process | danchip/QC/QCprocA, 55 cycles (11+44) or 10:05 minutes | S004580 | OLD showerhead | |
1/12-2014 | 4" Danchip QC Wafer | 1.5 µm AZ resist, daq2 mask | Si / 10 % | Pegasus/jmli | 10 minute TDESC clean, 10 minute PR strip post process | danchip/QC/QCprocA, 55 cycles (11+44) or 10:05 minutes | S004671 | New showerhead | |
15/12-2014 | 4" Danchip QC Wafer | 1.5 µm AZ resist, daq2 mask | Si / 10 % | Pegasus/jmli | 10 minute TDESC clean, 10 minute PR strip post process | danchip/QC/QCprocA, 55 cycles (11+44) or 10:05 minutes | S004746 | New showerhead |