===Deal-Grove parameters=== | |||
The following table contains linear and parabolic parameters for use in the Deal-Grove model for thermal oxidation. The parameters are obtained a least squares fit to data available in the furnace logbooks. Information on wafer orientation and doping concentration, which is not available in the logbooks, has not been included in calculating the parameters. | |||
{| class="wikitable" | |||
! | |||
! colspan="3" style="text-align: center;" | Anneal Oxide | |||
! colspan="3" style="text-align: center;" | Anneal Bond | |||
! colspan="3" style="text-align: center;" | Boron Drive-in | |||
! colspan="3" style="text-align: center;" | Gate Oxide | |||
! colspan="3" style="text-align: center;" | Phosphor Drive-in | |||
|- | |||
| style="text-align: center;" | Recipe | |||
| style="text-align: center;" | B [µm2/h] | |||
| style="text-align: center;" | B/A [µm/h] | |||
| RMSE [nm] | |||
| style="text-align: center;" | B [µm2/h] | |||
| style="text-align: center;" | B/A [µm/h] | |||
| style="text-align: center;" | RMSE [nm] | |||
| style="text-align: center;" | B [µm2/h] | |||
| style="text-align: center;" | B/A [µm/h] | |||
| RMSE [nm] | |||
| style="text-align: center;" | B [µm2/h] | |||
| style="text-align: center;" | B/A [µm/h] | |||
| RMSE [nm] | |||
| style="text-align: center;" | B [µm2/h] | |||
| style="text-align: center;" | B/A [µm/h] | |||
| RMSE [nm] | |||
|- | |||
| DRY900 | |||
| style="text-align: center;" | 0.000408 | |||
| style="text-align: center;" | 0.107 | |||
| style="text-align: center;" | Too little data | |||
| style="text-align: center;" | 0.0660 | |||
| style="text-align: center;" | 0.272 | |||
| style="text-align: center;" | 31 | |||
| style="text-align: center;" | 0.000390 | |||
| style="text-align: center;" | 0.154 | |||
| style="text-align: center;" | Too little data | |||
| style="text-align: center;" | 0.0028 | |||
| style="text-align: center;" | 0.079 | |||
| style="text-align: center;" | 4 (limited data) | |||
| style="text-align: center;" | 0.0507 | |||
| style="text-align: center;" | 0.884 | |||
| style="text-align: center;" | Too little data | |||
|- | |||
| DRY1000 | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | 0.465 | |||
| style="text-align: center;" | 0.838 | |||
| style="text-align: center;" | 20 | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | 0.641 | |||
| style="text-align: center;" | 1.45 | |||
| style="text-align: center;" | 41 | |||
|- | |||
| DRY1050 | |||
| style="text-align: center;" | 0.0111 | |||
| style="text-align: center;" | 0.526 | |||
| style="text-align: center;" | 27 | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | 0.0129 | |||
| style="text-align: center;" | 0.330 | |||
| style="text-align: center;" | 8 | |||
| style="text-align: center;" | 0.022 | |||
| style="text-align: center;" | 0.505 | |||
| style="text-align: center;" | 3 (limited data) | |||
| style="text-align: center;" | 0.0134 | |||
| style="text-align: center;" | 0.362 | |||
| style="text-align: center;" | 6 | |||
|- | |||
| DRY1100 | |||
| style="text-align: center;" | 0.020 | |||
| style="text-align: center;" | 0.930 | |||
| style="text-align: center;" | 10 | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | 0.0212 | |||
| style="text-align: center;" | 0.736 | |||
| style="text-align: center;" | 23 | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | 0.0313 | |||
| style="text-align: center;" | 0.553 | |||
| style="text-align: center;" | 14 | |||
|- | |||
| WET950 | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | 0.0716 | |||
| style="text-align: center;" | 1.25 | |||
| style="text-align: center;" | 12 | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | 0.110 | |||
| style="text-align: center;" | 1.17 | |||
| style="text-align: center;" | 11 | |||
|- | |||
| WET1000 | |||
| style="text-align: center;" | 0.192 | |||
| style="text-align: center;" | 1.54 | |||
| style="text-align: center;" | 44 | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | 0.192 | |||
| style="text-align: center;" | 1.80 | |||
| style="text-align: center;" | 29 | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | 0.195 | |||
| style="text-align: center;" | 2.49 | |||
| style="text-align: center;" | 22 | |||
|- | |||
| WET1050 | |||
| style="text-align: center;" | 0.487 | |||
| style="text-align: center;" | 0.965 | |||
| style="text-align: center;" | 29 | |||
| style="text-align: center;" | 0.477 | |||
| style="text-align: center;" | 0.899 | |||
| style="text-align: center;" | Too little data | |||
| style="text-align: center;" | 0.455 | |||
| style="text-align: center;" | 1.33 | |||
| style="text-align: center;" | 16 | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | 0.448 | |||
| style="text-align: center;" | 1.73 | |||
| style="text-align: center;" | 12 | |||
|- | |||
| WET1100 | |||
| style="text-align: center;" | 0.580 | |||
| style="text-align: center;" | 1.43 | |||
| style="text-align: center;" | 8 | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | 0.519 | |||
| style="text-align: center;" | 1.186 | |||
| style="text-align: center;" | 3 | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | - | |||
| style="text-align: center;" | 0.403 | |||
| style="text-align: center;" | 9.05 | |||
| style="text-align: center;" | 7 | |||
|} | |||
===Wet Oxidation on <100>=== | ===Wet Oxidation on <100>=== | ||
Revision as of 16:11, 22 January 2015
Feedback to this page: click here
Oxidation
At Danchip we have seven furnaces for oxidation: A1, A2, A3, C1, C3, D1 and Noble. Oxidation can take place either by a dry process or a wet process. The film quality of dry oxide is better than for wet oxide with regards to density and dielectric constant, however the oxidation rate is slow for dry oxide. If the film quality for the wet oxide is acceptable then the thickness and the time it takes to grow the oxide often decides if a dry or wet oxidation is chosen.
- Dry oxidation is used from 5 nm - 200 nm and can be grown in the furnaces: A1, A2, A3, C1, C3.
- Wet oxidation is used up to 4 µm and can be grown in the furnaces: A1, A3, Noble.
- Very thick oxide >4 µm can be grown in D1, it is still a wet oxidation.
The standard recipes, quality control limits and results for the Boron Drive-in + Predep furnace (A1) and the Phosphorus Drive-in furnace (A3) can be found here:
- Standard recipes, QC limits and results for the Boron Drive-in + Predep furnace (A1)
- Standard recipes, QC limits and results for the Phosphorus Drive-in furnace (A3)
- Wet oxidation in Anneal-oxide furnace (C1)
- Oxidation on III-V furnace (D4) - For oxidation of AlxGaAs layers.
Comparison of the seven oxidation furnaces
| Generel description | Drive-in of boron deposited in the same furnace or drive-in of ion implanted boron. Can also be used for dry and wet oxidation. | Oxidation of gate-oxide and other very clean oxides. | Drive-in of phosphorous deposited in the phosphorous pre-dep furnace (A4) or drive-in of ion implanted phosphorous. Can also be used for dry and wet oxidation. | Oxidation of 4" and 6" wafers. Oxidation of new wafers without RCA cleaning. Oxidation of wafers from the LPCVD furnaces and PECVD2. | Oxidation of wafers from EVG-NIL, PECVD3 and wafers with aluminum. | Oxidation of very thick oxides, thickness higher than 4 µm. | Oxidation of almost all materials on silicon wafers. |
|---|---|---|---|---|---|---|---|
| Oxidation method |
|
|
|
|
|
|
|
| Annealing gas |
|
|
|
|
|
|
|
| Process temperature |
|
|
|
|
|
|
|
| Substrate and Batch size |
Including one test wafer |
Including one test wafer |
Including one test wafer |
Including one test wafer |
Including one test wafer |
|
|
| Allowed materials |
All wafers have to be RCA cleaned, except for boron pre-doped wafers from the same furnace. |
All wafers have to be RCA cleaned. |
All wafers have to be RCA cleaned, except for phosphorous pre-doped wafers from furnace A4. |
All processed wafers have to be RCA cleaned, except for wafers from LPCVD furnaces and PECVD2. |
All wafers have to be RCA cleaned, except for wafers from EVG-NIL, PECVD3 and wafers with aluminum. |
Only new wafers |
Almost all materials, permission is needed |
Oxidation curves
Color chart for oxide/nitride thickness
Generic calculator for wet/dry oxide thickness calculation
The following links give an approximate oxide time/thickness based on a general formula:
Deal-Grove parameters
The following table contains linear and parabolic parameters for use in the Deal-Grove model for thermal oxidation. The parameters are obtained a least squares fit to data available in the furnace logbooks. Information on wafer orientation and doping concentration, which is not available in the logbooks, has not been included in calculating the parameters.
| Anneal Oxide | Anneal Bond | Boron Drive-in | Gate Oxide | Phosphor Drive-in | |||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Recipe | B [µm2/h] | B/A [µm/h] | RMSE [nm] | B [µm2/h] | B/A [µm/h] | RMSE [nm] | B [µm2/h] | B/A [µm/h] | RMSE [nm] | B [µm2/h] | B/A [µm/h] | RMSE [nm] | B [µm2/h] | B/A [µm/h] | RMSE [nm] |
| DRY900 | 0.000408 | 0.107 | Too little data | 0.0660 | 0.272 | 31 | 0.000390 | 0.154 | Too little data | 0.0028 | 0.079 | 4 (limited data) | 0.0507 | 0.884 | Too little data |
| DRY1000 | - | - | - | - | - | - | 0.465 | 0.838 | 20 | - | - | - | 0.641 | 1.45 | 41 |
| DRY1050 | 0.0111 | 0.526 | 27 | - | - | - | 0.0129 | 0.330 | 8 | 0.022 | 0.505 | 3 (limited data) | 0.0134 | 0.362 | 6 |
| DRY1100 | 0.020 | 0.930 | 10 | - | - | - | 0.0212 | 0.736 | 23 | - | - | - | 0.0313 | 0.553 | 14 |
| WET950 | - | - | - | - | - | 0.0716 | 1.25 | 12 | - | - | - | 0.110 | 1.17 | 11 | |
| WET1000 | 0.192 | 1.54 | 44 | - | - | 0.192 | 1.80 | 29 | - | - | - | 0.195 | 2.49 | 22 | |
| WET1050 | 0.487 | 0.965 | 29 | 0.477 | 0.899 | Too little data | 0.455 | 1.33 | 16 | - | - | - | 0.448 | 1.73 | 12 |
| WET1100 | 0.580 | 1.43 | 8 | - | - | - | 0.519 | 1.186 | 3 | - | - | - | 0.403 | 9.05 | 7 |
Wet Oxidation on <100>
The curves below are based on measurements in our specific furnaces and give more accurate results. We will still recommend to make minimum one test run if the thickness is very important.
- Wet oxidation
-
A1 Furnace <100>-Si Wet Oxidation
-
A3 Furnace <100>-Si Wet Oxidation
Dry Oxidation on <100> and <111> wafer
- Dry oxidation
-
Dry oxide on <100> wafer. The y-axis is in Å and the x-axis is in minutes.
-
Dry oxide on <111> wafer. The y-axis is in Å and the x-axis is in minutes.