The procedure is as follows:
The procedure is as follows:


====When deposition on one side of the wafer:====
==When deposition on one side of the wafer==
#Measure the wafer bow on one of the profilometers (Tencor or Dektak 8). Save the measurement. It is a good idea to measure across most of the wafer in two directions perpendicular to each other.
#Measure the wafer bow on one of the profilometers (Tencor or Dektak 8). Save the measurement. It is a good idea to measure across most of the wafer in two directions perpendicular to each other.
#Deposite the thin film
#Deposite the thin film
Line 14: Line 14:
#Use the program for stress measurement in the profilometer software on the profilometer you used for the measurements. Use both the pre-stress measurement and the post-stress measurement.
#Use the program for stress measurement in the profilometer software on the profilometer you used for the measurements. Use both the pre-stress measurement and the post-stress measurement.


====When deposition on both sides of the wafer:====
==When deposition on both sides of the wafer==
#Deposite the thin film
#Deposite the thin film
#Pre-measurement: Measure the wafer bow on one of the profilometers (Tencor or Dektak 8). Save the measurement. It is a good idea to measure across most of the wafer in two directions perpendicular to each other.  
#Pre-measurement: Measure the wafer bow on one of the profilometers (Tencor or Dektak 8). Save the measurement. It is a good idea to measure across most of the wafer in two directions perpendicular to each other.  

Revision as of 15:19, 31 January 2008

Stress measurements of a thin film can be done measuring the wafer bow before and after deposition of the film. If the film is deposited on both sides of the wafer you can measure the bow after deposition and again after removing the film from one of the sides.

The procedure is as follows:

When deposition on one side of the wafer

  1. Measure the wafer bow on one of the profilometers (Tencor or Dektak 8). Save the measurement. It is a good idea to measure across most of the wafer in two directions perpendicular to each other.
  2. Deposite the thin film
  3. Measure the wafer bow again:
    • On the same profilometer as used for the pre-measurement.
    • With the same recipe as used for the pre-mesurement.
    • On the same position/positions on the wafer as the pre-measurement .
  4. Measure the thickness of the substrate
  5. Measure the thickness of the thin film (ex. using the FilmTek or the Ellipsometer is possible).
  6. Use the program for stress measurement in the profilometer software on the profilometer you used for the measurements. Use both the pre-stress measurement and the post-stress measurement.

When deposition on both sides of the wafer

  1. Deposite the thin film
  2. Pre-measurement: Measure the wafer bow on one of the profilometers (Tencor or Dektak 8). Save the measurement. It is a good idea to measure across most of the wafer in two directions perpendicular to each other.
  3. Remove the thin film from one side of the wafer. If it is a single side polished wafer, remove it on the non-polished side.
  4. Measure the wafer bow again:
    • On the same profilometer as used for the pre-measurement.
    • With the same recipe as used for the pre-mesurement.
    • On the same position/positions on the wafer as the pre-measurement .
  5. Measure the thickness of the substrate
  6. Measure the thickness of the thin film (ex. using the FilmTek or the Ellipsometer is possible).
  7. Use the program for stress measurement in the profilometer software on the profilometer you used for the measurements. Use both the pre-stress measurement and the post-stress measurement.