KOH belongs to the family of anisotropic Si-etchants based on aqueous alkaline solutions. The anisotropy stems from the different etch rates in different crystal directions. The {111}-planes are almost inert whereas the etch rates of e.g. {100}- and {110}-planes are several orders of magnitude faster.
KOH belongs to the family of anisotropic Si-etchants based on aqueous alkaline solutions. The anisotropy stems from the different etch rates in different crystal directions. The {111}-planes are almost inert whereas the etch rates of e.g. {100}- and {110}-planes are several orders of magnitude faster.


KOH-etching is a highly versatile and cheap way to realize micro mechanical structures if you can live with the necessary Si<math>_3</math>N<math>_4</math>- or SiO<math>_2</math>-masking materials and the potassium contamination of the surface. The latter necessitates in most cases a wet post-clean ('7-up' or RCA-clean) if the wafer is to be processed further.
KOH-etching is a highly versatile and cheap way to realize micro mechanical structures if you can live with the necessary Si<math>_3</math>N<math>_4</math>- or SiO<math>_2</math>-masking materials and the potassium contamination of the surface. The latter necessitates in most cases a wet post-clean ([[Specific Process Knowledge/Wafer cleaning/7-up & Piranha|'7-up']] or [[Specific Process Knowledge/Wafer cleaning/RCA|RCA-clean]] if the wafer is to be processed further.


At Danchip we use as a standard a 28 wt% KOH. The etch rate - and the selectivity towards a SiO<math>_2</math>-mask - is depending on the temperature. We normally use T=80 <sup>o</sup>C but may choose to reduce this to e.g. 60 <sup>o</sup>C or 70 <sup>o</sup>C in case of a high-precision timed etch (e.g. defining a thin membrane). In some cases we recommend to saturate the standard 28 wt% KOH with IPA with an etch temperature at T=70 <sup>o</sup>C (reduce evaporation of IPA). One example is for boron etch-stop, where the selectivity towards the boron-doped silicon is improved compared to the standard etch. Key facts for the two solutions are resumed in the table:
At Danchip we use as a standard a 28 wt% KOH. The etch rate - and the selectivity towards a SiO<math>_2</math>-mask - is depending on the temperature. We normally use T=80 <sup>o</sup>C but may choose to reduce this to e.g. 60 <sup>o</sup>C or 70 <sup>o</sup>C in case of a high-precision timed etch (e.g. defining a thin membrane). In some cases we recommend to saturate the standard 28 wt% KOH with IPA with an etch temperature at T=70 <sup>o</sup>C (reduce evaporation of IPA). One example is for boron etch-stop, where the selectivity towards the boron-doped silicon is improved compared to the standard etch. Key facts for the two solutions are resumed in the table:

Revision as of 14:19, 21 February 2008

KOH etch - Anisotropic silicon etch

KOH etch for 4" wafers: positioned in cleanroom 3

KOH belongs to the family of anisotropic Si-etchants based on aqueous alkaline solutions. The anisotropy stems from the different etch rates in different crystal directions. The {111}-planes are almost inert whereas the etch rates of e.g. {100}- and {110}-planes are several orders of magnitude faster.

KOH-etching is a highly versatile and cheap way to realize micro mechanical structures if you can live with the necessary Si3N4- or SiO2-masking materials and the potassium contamination of the surface. The latter necessitates in most cases a wet post-clean ('7-up' or RCA-clean if the wafer is to be processed further.

At Danchip we use as a standard a 28 wt% KOH. The etch rate - and the selectivity towards a SiO2-mask - is depending on the temperature. We normally use T=80 oC but may choose to reduce this to e.g. 60 oC or 70 oC in case of a high-precision timed etch (e.g. defining a thin membrane). In some cases we recommend to saturate the standard 28 wt% KOH with IPA with an etch temperature at T=70 oC (reduce evaporation of IPA). One example is for boron etch-stop, where the selectivity towards the boron-doped silicon is improved compared to the standard etch. Key facts for the two solutions are resumed in the table:


KOH solutions

28 wt% KOH 28 wt% KOH sat. with IPA
General description
Etch of Si(100)
Etch of Si(100) with boron etch-stop
Chemical solution
KOH:H2O - 500 g : 1000 ml
KOH:H2O:IPA - 500 g : 1000 ml : ?? ml
Process temperature
  • 60 oC
  • 70 oC
  • 80 oC (standard - fast etch)
  • 70 oC
Possible masking materials
  • Stoichiometric Si3N4
  • Si-rich Si3N4
  • PECVD Si3N4
  • Thermal SiO2
  • Stoichiometric Si3N4
  • Si-rich Si3N4
  • PECVD Si3N4
  • Thermal SiO2
Etch rate
  • ~0.4 µm/min (60 oC)
  • ~0.7 µm/min (70 oC)
  • ~1.3 µm/min (80 oC)
  • ~0.2 µm/min (70 oC)
in p++ (doping level > 5x1019 cm-3)
Roughness
Typical: 100-600 Å
May form hillocks (pyramidal)
Batch size
1-25 wafers at a time
1-25 wafer at a time
Size of substrate
4" wafers
4" wafers
Allowed materials
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride


Definition of structures

Due to the almost inert (111)-planes.....


Definition of <110> alignment structures

The etch rate dependence on the crystallographic planes can be used to determine the <110> crystal directions with high precision (better than +/- 0.05 o). A fast method for doing this, using the symmetric under-etching behavior around but not at the <110>-directions, was described by Vangbo and Bäcklund in J. Micromech. Microeng.6 (1996), 279-284. High-precision control of the <110>-direction during alignment can be necessary in order to control the dimensions of KOH-etched structures (e.g. precise control of V-groove dimensions). A dedicated mask (MASK NAME) has been designed for this purpose.


Etch rates: Empirical formula (Seidl et al)

The following empirical formula can be used for concentrations in the range of 10-60 wt%:

R = k0 [H2O]4 [KOH]0.25 e-Ea/kT,

where k0 = 2480 µm/hr (mol/l)-4.25, Ea = 0.595 eV for Si(100)

and k0 = 4500 µm/hr (mol/l)-4.25, Ea = 0.60 eV for Si(110)