Specific Process Knowledge/Lithography/Baking: Difference between revisions
| Line 35: | Line 35: | ||
[[Image:Oven_90_degrees_cr3.jpg|300x300px|thumb|Oven 90 °C: positioned in C-1]] | [[Image:Oven_90_degrees_cr3.jpg|300x300px|thumb|Oven 90 °C: positioned in C-1]] | ||
The oven is mostly used for baking of several wafers at a time at 90 °C as a soft baking step after a spin coating of photoresist. For 1.5µm resist the baking time is 30 min. For most of the other resist thicknesses it is also 30 min. | The oven is mostly used for baking of several wafers at a time at 90 °C as a soft baking step after a spin coating of photoresist. For 1.5µm resist the baking time is 30 min. For most of the other resist thicknesses it is also 30 min. | ||
<br clear="all" /> | <br clear="all" /> | ||
Revision as of 13:13, 23 October 2014
Feedback to this page: click here
Hotplates
90 C 4" hotplate

This hotplate is mostly used for baking of single wafers at 90 °C as a soft baking step after a spin coating of photoresist.
110 C 4" hotplate

The 110 °C hotplate is used for 2 different things; hard bake of resist, and image reversal baking between two exposures. It is recommended to hard bake for 2 min. For image reversal it is recommended to bake at least 100 sec., some bake for 120 sec.
Hotplate: 90-110C

Hotplate: 90-110C is used for baking of 2" - 6" wafers.
The user manual, and contact information can be found in LabManager: Hotplate: 90-110C
SU8 hotplates

We have two dedicated SU-8 hotplates in C-1.
Users can control the ramp-time, the baking temperature, and the baking time.
The user manual, and contact information can be found in LabManager: Hotplate 1 (SU8) Hotplate 2 (SU8)
Ovens
90 C oven

The oven is mostly used for baking of several wafers at a time at 90 °C as a soft baking step after a spin coating of photoresist. For 1.5µm resist the baking time is 30 min. For most of the other resist thicknesses it is also 30 min.
120 C oven

120 °C oven is used to hard bake of resist on several wafers at time. It is recommended to hard bake for 30 min.
250 C oven for pretreatment

The oven is typically used for pretreatment of silicon and glass substrates to promote the resist adhesion. We recommend to place the wafers in metal carrier in the oven at least for 4 hours, even better over night, and spin the resist on them asap.
The user manual, and contact information can be found in LabManager: Oven 250C
250 C oven for burning resist

This oven is used for "burning" the resist, therefore not considered clean.