[[image:EDX-scheme.jpg|250x250px|right|thumb|The high energy electrons in the beam (denoted above as incident particle) collide with the core electrons of the sample atoms that are left in an excited state with higher energy. One decay mechanism is to let an outer electron fall into the unoccupied state under emission of a photon that carries the excess energy. This energy is determined by the electronic shells and hence characteristic of the atom.]]
You can make detailed analysis on the elemental composition and distribution in a sample with 3 instruments at Danchip. The [[Specific Process Knowledge/Characterization/SEM: Scanning Electron Microscopy/Leo|Leo SEM]] and [[Specific Process Knowledge/Characterization/SEM: Scanning Electron Microscopy/FEI|FEI SEM]] are both equipped with an X-ray detector that allows you to make elemental analysis by using the technique Energy Dispersive X-ray analysis or EDX. The [[Specific Process Knowledge/Characterization/SIMS: Secondary Ion Mass Spectrometry|Atomika SIMS]] uses a technique called Secondary Ion Mass Spectrometry or SIMS.
You can make detailed analysis on the elemental composition and distribution in a sample with 3 instruments at Danchip. The [[Specific Process Knowledge/Characterization/SEM: Scanning Electron Microscopy/Leo|Leo SEM]] and [[Specific Process Knowledge/Characterization/SEM: Scanning Electron Microscopy/FEI|FEI SEM]] are both equipped with an X-ray detector that allows you to make elemental analysis by using the technique Energy Dispersive X-ray analysis or EDX. The [[Specific Process Knowledge/Characterization/SIMS: Secondary Ion Mass Spectrometry|Atomika SIMS]] uses a technique called Secondary Ion Mass Spectrometry or SIMS.


Line 15: Line 13:


== Secondary Ion Mass Spectrometry ==
== Secondary Ion Mass Spectrometry ==
[[image:SIMScascade.gif|250x250px|right|thumb|A beam of high energy ions is rastered on the surface of the sample. Some of the atoms that used to make up the surface are sputtered off and emitted as secondary ions. The mass of the these ions is measured with a mass spectrometer.]]


In the Atomika SIMS the samples are bombarded with a beam of either oxygen or caesium ions. When accelerated to high energy and rastered across the sample
In the Atomika SIMS the samples are bombarded with a beam of either oxygen or caesium ions. When accelerated to high energy and rastered across the sample

Revision as of 16:25, 30 January 2008

You can make detailed analysis on the elemental composition and distribution in a sample with 3 instruments at Danchip. The Leo SEM and FEI SEM are both equipped with an X-ray detector that allows you to make elemental analysis by using the technique Energy Dispersive X-ray analysis or EDX. The Atomika SIMS uses a technique called Secondary Ion Mass Spectrometry or SIMS.

Energy Dispersive X-ray analysis

The technique of extracting information from the X-rays generated in a sample that is irradiated with electrons is called energy dispersive X-ray analysis or EDX. (Other acronyms are Energy Dispersive x-ray Spectroscopy, EDS, or Electron Probe Microanalysis, EPMA). The energetic electrons in the incident beam create core level vacancies as they collide with sample atoms electrons in a multiple scattering process. This leaves the atoms in the sample in an excited state. In the process of decaying from this state photons may be emitted. The energy of these photons is determined by the difference in energy of the shells involved. Since atomic shells are unique for every element so will be the transitions between them. Thus, every element has its own characteristic X-ray spectrum that can be used to determine the elemental composition.

Adding an EDX detector to a SEM provides a very powerful tool for elemental analysis. The capability of the SEM to precisely maneuver the electron beam in a number of ways enables us to make point-like analysis with nanometer precision.

Secondary Ion Mass Spectrometry

In the Atomika SIMS the samples are bombarded with a beam of either oxygen or caesium ions. When accelerated to high energy and rastered across the sample these ions will be able to gradually sputter off the surface atoms in a small area defined by the raster pattern. Some of the surface atoms are emitted as ionized particles. In this way one layer after another is peeled off the sample.

These charged species are led through a mass spectrometer where a magnetic field is used to deflect them. The deflection increases with charge and decreases with mass and we are therefore able detect and count them according to their mass. This technique is called Secondary Ion Mass Spectrometry or SIMS.

SEM with EDX SIMS
Full name Energy Dispersive X-ray Analysis Secondary Ion Mass Spectroscopy
Technique Non destructive method: X-rays are generated when the primary beam impinge on the sample. The elemental analysis is possible because the energy of these photons is characteristic of the element they emitted from. Destructive method: A beam of high energy heavy ions (caesium or oxygen) sputters off surface atoms that are subsequently measured with a mass spectrometer.
What elements are detected Every element heavier than boron/carbon Every element
Chemical information None: Only transistions involving inner shell electrons are detected None
Sample limitations Vacuum compatible. Vacuum compatible. The sample needs to be cut into small (app. 5*5 mm) pieces.
Spatial resolution Very precise point-like analysis is possible with SEM electron beam. Limited to what is visible in a camera
Depth resolution The size interaction volume depends on the SEM high voltage and sample density: The higher the SEM high voltage the bigger and deeper the interaction volume. The more dense the material is the smaller is the interaction volume. The sputtering of the surface makes it possible to perform detailed depth profiling with extremely good sensitivity and depth resolution.
Detection limit Approximately 1 % atomic weight Down to 1 ppb for many elements
Speed of measurement Quite fast and easy Time consuming

The technique is highly sensitive and is therefore ideal if you want to check for a contamination. In a typical application one puts three samples into the SIMS.

Depth resolution using EDX