Jump to content

Specific Process Knowledge/Etch/Wet Polysilicon Etch: Difference between revisions

From LabAdviser
Line 36: Line 36:
|Etch rate
|Etch rate
|
|
*~85 Å/min (stoichiometric Si<sub>3</sub>N<sub>4</sub>)
*R<sub>Si</sub> ~1000-2000 Å/min (depending on doping level)
*~60 Å/min (si-rich Si<sub>3</sub>N<sub>4</sub>)
*~60 Å/min (si-rich Si<sub>3</sub>N<sub>4</sub>)
*~30 Å/min (annealed si-rich Si<sub>3</sub>N<sub>4</sub>)
*~30 Å/min (annealed si-rich Si<sub>3</sub>N<sub>4</sub>)

Revision as of 13:26, 30 January 2008

Wet Poly Etch

Wet PolySilicon Etch (in the middle): positioned in cleanroom 4

The wet Poly Etch is an isotropic silicon etch. This holds for both a poly-silicon thin-film as well as single-crystalline material such as a Si(100) surface. The Poly Etch process is placed in a dedicated PP-tank in a laminar-flow bench in cleanroom 4.

The Poly Etch is typically used for opening holes in poly-silicon thin-films, using photoresist as an etch mask. Due to its isotropic nature the under-etching (etch-bias) at least amounts to the thickness of the poly-silicon layer. Another example of usage is etching of "circular-shaped" holes in silicon substrates.

The Poly Etch is based on the combined oxidation of silicon followed by dissolution of the silicon oxide. The etch solution consists of:

HNO3 : BHF : H2O (20 : 1 : 20)


Poly Etch data

Poly Etch @ room temperature
General description

Etch of poly-si/Si(100)

Chemical solution HNO3 : BHF : H2O (20 : 1 : 20)
Process temperature Room temperature
Possible masking materials:
  • Photoresist(min. 2.2 µm is recommended)
  • LPCVD-oxide (TEOS)
Etch rate
  • RSi ~1000-2000 Å/min (depending on doping level)
  • ~60 Å/min (si-rich Si3N4)
  • ~30 Å/min (annealed si-rich Si3N4)
  • ~4 Å/min (Thermal oxide)
Batch size

1-25 wafers at a time

Size of substrate

2-6" wafers