The Poly Etch is based on the combined oxidation of silicon followed by dissolution of the silicon oxide. The etch solution consists of:
The Poly Etch is based on the combined oxidation of silicon followed by dissolution of the silicon oxide. The etch solution consists of:


HNO<sub>3</sub> : BHF : H<sub>2</sub>O                                       20 : 1 : 20
HNO<sub>3</sub> : BHF : H<sub>2</sub>O   (20 : 1 : 20)




Line 23: Line 23:
|-
|-
|Chemical solution
|Chemical solution
|H<sub>3</sub>PO<sub>4</sub>     (85 wt%)
|HNO<sub>3</sub> : BHF : H<sub>2</sub>(20 : 1 : 20)
 
|-
|-
|Process temperature
|Process temperature
|180 <sup>o</sup>C
|Room temperature
|-
|-
|Possible masking materials:
|Possible masking materials:
|
|
*Thermal oxide (converted si-rich surface)
*Photoresist(min. 2.2 µm is recommended)
*LPCVD-oxide (TEOS)
*LPCVD-oxide (TEOS)
*PECVD-oxide
|-
|-
|Etch rate
|Etch rate

Revision as of 13:12, 30 January 2008

Wet Poly Etch

Wet PolySilicon Etch (in the middle): positioned in cleanroom 4

The wet Poly Etch is an isotropic silicon etch. This holds for both a poly-silicon thin-film as well as single-crystalline material such as a Si(100) surface. The Poly Etch process is placed in a dedicated PP-tank in a laminar-flow bench in cleanroom 4.

The Poly Etch is typically used for opening holes in poly-silicon thin-films, using photoresist as an etch mask. Due to its isotropic nature the under-etching (etch-bias) at least amounts to the thickness of the poly-silicon layer. Another example of usage is etching of "circular-shaped" holes in silicon substrates.

The Poly Etch is based on the combined oxidation of silicon followed by dissolution of the silicon oxide. The etch solution consists of:

HNO3 : BHF : H2O (20 : 1 : 20)


Poly Etch data

Poly Etch @ room temperature
General description

Etch of poly-si/Si(100)

Chemical solution HNO3 : BHF : H2O (20 : 1 : 20)
Process temperature Room temperature
Possible masking materials:
  • Photoresist(min. 2.2 µm is recommended)
  • LPCVD-oxide (TEOS)
Etch rate
  • ~85 Å/min (stoichiometric Si3N4)
  • ~60 Å/min (si-rich Si3N4)
  • ~30 Å/min (annealed si-rich Si3N4)
  • ~4 Å/min (Thermal oxide)
Batch size

1-25 wafers at a time