|-style="background: | |-style="background:green; color:White" | ||
!colspan="7"|AllResist CSAR | !colspan="7"|AllResist CSAR on Spin Coater: Manual LabSpin A-5, TIGRE, 16-06-2014. Softbake 2 min @ 150 degC. | ||
|- | |- | ||
| Line 194: | Line 197: | ||
!Thickness [nm] | !Thickness [nm] | ||
!St Dev | !St Dev | ||
|- | |- | ||
| Line 208: | Line 203: | ||
|3000 | |3000 | ||
|4000 | |4000 | ||
| | |201.61 | ||
| | |1.20 | ||
|- | |- | ||
| Line 216: | Line 211: | ||
|4000 | |4000 | ||
|4000 | |4000 | ||
| | |173.89 | ||
|0. | |0.64 | ||
|- | |- | ||
| Line 224: | Line 219: | ||
|5000 | |5000 | ||
|4000 | |4000 | ||
| | |155.91 | ||
|0. | |0.65 | ||
|- | |- | ||
|} | |} | ||
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 40%" | {|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" style="width: 40%" | ||
| Line 244: | Line 230: | ||
|- | |- | ||
|-style="background: | |-style="background:red; color:White" | ||
!colspan="7"|AllResist CSAR | !colspan="7"|AllResist CSAR 1:1 in anisole, Spin Coater: Manual LabSpin A-5, TIGRE, 16-06-2014. Softbake 2 min @ 150 degC. | ||
|- | |- | ||
| Line 254: | Line 240: | ||
!Thickness [nm] | !Thickness [nm] | ||
!St Dev | !St Dev | ||
|- | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
|2000 | |||
|4000 | |||
|83.48 | |||
|0.49 | |||
|- | |- | ||
| Line 260: | Line 254: | ||
|3000 | |3000 | ||
|4000 | |4000 | ||
| | |67.12 | ||
| | |0.41 | ||
|- | |- | ||
| Line 268: | Line 262: | ||
|4000 | |4000 | ||
|4000 | |4000 | ||
| | |58.64 | ||
|0. | |0.44 | ||
|- | |- | ||
| Line 276: | Line 270: | ||
|5000 | |5000 | ||
|4000 | |4000 | ||
| | |53.13 | ||
|0. | |0.39 | ||
|- | |- | ||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
|6000 | |||
|4000 | |||
|48.76 | |||
|0.38 | |||
|- | |||
|} | |} | ||
Revision as of 16:00, 16 June 2014
These tests are currently in progress and this page thus under construction. If you have questions to the process or wish to use this e-beam resist, please contact Tine Greibe at tigre@danchip.dtu.dk.
Process Flow
Test of Chemically Semi-Amplified Resist (CSAR); a positive e-beam resist from AllResist (AR-P 6200-2).
| Equipment | Process Parameters | Comments | Initials and date |
|---|---|---|---|
| Pretreatment | |||
| 4" Si wafers | No Pretreatment | TIGRE, 08-04-2014 | |
| Spin Coat | |||
| Spin Coater Manual, LabSpin, A-5 | AR-P 6200/2 AllResist E-beam resist
60 sec at various spin speed. Acceleration 4000 s-2, softbake 2 - 5 min at 150 deg Celcius |
Resist poured directly from bottle | TIGRE, 09-04-2014, 16-06-2014 |
| Characterization | |||
| Ellipsometer VASE B-1 | 9 points measured on 100 mm wafer | ZEP program used; measured at 70 deg only | TIGRE, 09-04-2014 |
| E-beam Exposure | |||
| JEOL 9500 E-beam writer, E-1 | Dosepattern 14nm - 100nm,
dose 120-280 muC/cm2 |
Virtual chip mark height detection | TIGRE, 10-04-2014 |
| Development | |||
| Fumehood, D-3 | 60 sec in X AR 600-54/6,
60 sec rinse in IPA, N2 Blow dry |
Agitation (by hand) while developing | TIGRE, 10-04-2014 |
| Characterization | |||
| Zeiss SEM Supra 60VP, D-3 | TIGRE, ??-04-2014 | ||
Spin Curve

The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on Si. The measurements are performed at one incidence angle (70 degrees) only. 9 points on each 4" wafer has been measured; the standard deviation thus representing the homogeinity of the film on the 4" wafers.
| AllResist AR-P 6200/2 spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 09-04-2014. Softbake 5 min @ 150 degC. | ||||||
|---|---|---|---|---|---|---|
| Spin Speed [rpm] | Acceleration [1/s2] | Thickness [nm] | St Dev | |||
| 2000 | 4000 | 225.98 | 0.97 | |||
| 3000 | 4000 | 194.00 | 0.6 | |||
| 4000 | 4000 | 169.57 | 0.32 | |||
| 5000 | 4000 | 151.47 | 0.26 | |||
| 6000 | 4000 | 142.38 | 0.41 | |||
| 7000 | 4000 | 126.59 | 0.36 | |||
| AllResist CSAR on Spin Coater: Manual LabSpin A-5, TIGRE, 16-06-2014. Softbake 2 min @ 150 degC. | ||||||
|---|---|---|---|---|---|---|
| Spin Speed [rpm] | Acceleration [1/s2] | Thickness [nm] | St Dev | |||
| 3000 | 4000 | 201.61 | 1.20 | |||
| 4000 | 4000 | 173.89 | 0.64 | |||
| 5000 | 4000 | 155.91 | 0.65 | |||
| AllResist CSAR 1:1 in anisole, Spin Coater: Manual LabSpin A-5, TIGRE, 16-06-2014. Softbake 2 min @ 150 degC. | ||||||
|---|---|---|---|---|---|---|
| Spin Speed [rpm] | Acceleration [1/s2] | Thickness [nm] | St Dev | |||
| 2000 | 4000 | 83.48 | 0.49 | |||
| 3000 | 4000 | 67.12 | 0.41 | |||
| 4000 | 4000 | 58.64 | 0.44 | |||
| 5000 | 4000 | 53.13 | 0.39 | |||
| 6000 | 4000 | 48.76 | 0.38 | |||