{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" width="95%"
|-
|-
|-style="background:silver; color:black"
|'''Resist'''
|'''Polarity'''
|'''Manufacturer'''
|'''Comments'''
|'''Technical reports'''
|'''Spinner'''
|'''Developer'''
|'''Rinse'''
|'''Remover'''
|'''Process flows (in docx-format)'''
|-
|-
|-style="background:LightGrey; color:black"
|'''[[Specific_Process_Knowledge/Lithography/ZEP520A|ZEP520A]]'''
|Positive
|ZEON
|Positive resist
|[[media:ZEP520A.pdf|ZEP520A.pdf]], [[media:ZEP520A.xls|ZEP520A spin curves on SSE Spinner]]
|[[Specific_Process_Knowledge/Lithography/Coaters#SSE Spinner|SSE]], [[Specific_Process_Knowledge/Lithography/Coaters#Manual Spinner 1|Manual Spinner 1 (Laurell)]], [[Specific_Process_Knowledge/Lithography/Coaters#Spin_coater:_Manual_Labspin|Spin Coater Labspin]]
|ZED-N50/Hexyl Acetate,n-amyl acetate, oxylene. [[media:JJAP-51-06FC05.pdf‎|JJAP-51-06FC05.pdf‎]], [[media:JVB001037.pdf‎|JVB001037.pdf‎]]
|IPA
|acetone/1165
|[[media:Process_Flow_ZEP.docx|Process_Flow_ZEP.docx]], [[media:Process_Flow_ZEP_with_Al.docx‎|Process_Flow_ZEP_with_Al.docx‎]]
|}
These tests are currently in progress and this page thus under construction. If you have questions to the process or wish to use this e-beam resist, please contact Tine Greibe at tigre@danchip.dtu.dk.
These tests are currently in progress and this page thus under construction. If you have questions to the process or wish to use this e-beam resist, please contact Tine Greibe at tigre@danchip.dtu.dk.



Revision as of 10:01, 14 July 2014

Resist Polarity Manufacturer Comments Technical reports Spinner Developer Rinse Remover Process flows (in docx-format)
ZEP520A Positive ZEON Positive resist ZEP520A.pdf, ZEP520A spin curves on SSE Spinner SSE, Manual Spinner 1 (Laurell), Spin Coater Labspin ZED-N50/Hexyl Acetate,n-amyl acetate, oxylene. JJAP-51-06FC05.pdf‎, JVB001037.pdf‎ IPA acetone/1165 Process_Flow_ZEP.docx, Process_Flow_ZEP_with_Al.docx‎


These tests are currently in progress and this page thus under construction. If you have questions to the process or wish to use this e-beam resist, please contact Tine Greibe at tigre@danchip.dtu.dk.


Process Flow

Test of ZEP resist; a positive e-beam resist from ZEON.


Equipment Process Parameters Comments Initials and date
Pretreatment
4" Si wafers No Pretreatment TIGRE, 23-04-2014
Spin Coat
Spin Coater Manual, LabSpin, A-5 ZEP520A 1:1 or ZEP520A 1:2 E-beam resist

60 sec at various spin speed. Acceleration 4000 s-2, softbake 2 min at 180 deg Celcius

Resist poured directly from bottle or by use of disposable pipette1 TIGRE, 23-04-2014, 21-05-2014
Characterization
Ellipsometer VASE B-1 9 points measured on 100 mm wafer ZEP program used; measured at 70 deg only TIGRE, 23-04-2014, 21-05-2014
E-beam Exposure
JEOL 9500 E-beam writer, E-1 Dosepattern 14nm - 100nm,

dose 120-280 muC/cm2

Virtual chip mark height detection2 TIGRE
Development
Fumehood, D-3 60 sec in N50,

60 sec rinse in IPA, N2 Blow dry

Agitation (by hand) while developing TIGRE, XX-04-2014
Characterization
Zeiss SEM Supra 60VP, D-3 TIGRE, ??-04-2014

1 The disposable pipettes are not cleanroom compatible and must therefore be handled with care inside the cleanroom. Each bag contain 10 pipettes; the bags must be opened inside a fumehood and each pipette must be cleaned with a N2 gun before use.

2 The e-beam writer measures the height of the substrate and adjust the focus accordingly. This requires no actual chip marks on the wafer. See e-beam writer manual.

Spin Curves


The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on a Si wafer with native oxide. The measurements are performed at one incidence angle (70 degrees) only. 9 points on each 4" wafer has been measured; the standard deviation thus represents the homogeinity of the film on the 4" wafers.

ZEON ZEP520A1:1 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 23-04-2014. Resist was mixed 13-01-2014, i.e. approximatley 3 months old.
Spin Speed [rpm] Acceleration [1/s2] Thickness [nm] St Dev
3000 4000 111.29 0.65
4000 4000 95.17 2.16
5000 4000 87.23 0.81


ZEON ZEP520A1:1 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 21-05-2014. Resist was mixed 15-05-2014, i.e. approximatley 6 days old.
Spin Speed [rpm] Acceleration [1/s2] Thickness [nm] St Dev
2000 4000 141.03 1.02
3000 4000 115.96 0.98
4000 4000 100.56 0.80
5000 4000 91.01 0.38
6000 4000 84.85 0.37


ZEON ZEP520A1:2 in anisole spinning on Spin Coater: Manual LabSpin A-5, TIGRE, 21-05-2014. Resist was mixed 15-05-2014, i.e. approximatley 6 days old.
Spin Speed [rpm] Acceleration [1/s2] Thickness [nm] St Dev
2000 4000 79.12 1.74
3000 4000 64.30 0.34
4000 4000 55.50 0.48
5000 4000 50.53 0.62
6000 4000 46.34 1.01